Method for preparing direct reduced iron by utilizing metallurgical dust and sludge and direct reduced iron
Through the pretreatment of metallurgical dust sludge and the rotary kiln reduction and roasting process, the recovery rate of iron-containing materials in metallurgical dust sludge is improved, the problems of resource waste and blast furnace stability in metallurgical dust sludge treatment are solved, and the direct effect of high metallization rate is achieved Reduced iron production.
Patent Information
- Application Number
- CN202410820193.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-06-24
AI Technical Summary
The treatment methods of metallurgical dust sludge are mainly stored, landfill and direct sintering, which leads to waste of resources and blast furnace stability problems. The recovery rate of iron-containing materials is low, so it is necessary to improve the recovery rate of iron-containing materials in metallurgical dust sludge. .
By pretreating the metallurgical dust sludge, mixing with auxiliary materials and fuel at a specific mass ratio, reducing calcination in the rotary kiln is carried out, temperature and proportion are controlled to improve the reduction reaction, and direct reduction iron is prepared.
It improves the recovery rate of iron-containing materials in metallurgical dust sludge, produces direct reduced iron with a metallization rate of ≥75%, which has low cost and environmental protection advantages, and is suitable for steelmaking and blast furnace materials.
Smart Images

Figure CN118910350A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of metallurgical technology, and in particular to a method for preparing direct reduced iron using metallurgical dust and sludge, and direct reduced iron. Background Art
[0002] Metallurgical dust and sludge is one of the most important solid waste emissions in iron and steel metallurgy, with a production volume of about 100-130kg / t·steel. It is mainly produced by the dry or wet dust removal of atmospheric pollutants such as flue gas and dust, or the treatment of wastewater generated in the metallurgical process. Compared with smelting slag, the technology for the disposal of metallurgical dust and sludge started later, but due to its large output, the high iron content of some dust and sludge, and the high added value of utilization, it has also become an important field for the utilization of metallurgical solid waste and the development of circular economy.
[0003] At present, the treatment methods for metallurgical dust and mud are mainly based on stockpiling, landfill covering and returning to the blast furnace for sintering. Stockpiling treatment not only occupies a large amount of land and pollutes the ecological environment, but also causes a large amount of resource waste. If it is simply treated by direct sintering or pelletizing process and then enters the blast furnace again, it will cause the zinc and other metal elements in the dust and mud to circulate and enrich in the blast furnace, which will have an adverse effect on the iron-containing charge, coke and furnace lining refractory materials, thereby destroying the stable and smooth operation of the blast furnace, shortening the service life of the blast furnace, and increasing the production cost of the enterprise. At the same time, the recovery rate of iron-containing materials in metallurgical dust and mud is low after being simply treated by direct sintering or pelletizing process and then entering the blast furnace again. Therefore, while utilizing metallurgical dust and mud, improving the recovery rate of iron-containing materials in metallurgical dust and mud is a technical problem that urgently needs to be solved. Summary of the invention
[0004] The present application provides a method for preparing direct reduced iron using metallurgical dust and direct reduced iron, so as to solve the following technical problem: how to improve the recovery rate of iron-containing materials in metallurgical dust while utilizing metallurgical dust.
[0005] In a first aspect, the present application provides a method for preparing direct reduced iron using metallurgical dust and sludge, the method comprising:
[0006] Pre-treating metallurgical dust and mud to obtain raw materials;
[0007] The raw material, auxiliary material and fuel are mixed according to a set mass ratio to obtain a mixture; in the mixture, the content of TFe is 34% to 38%, and the content of C is 20% to 30% by mass fraction;
[0008] The mixed material is subjected to reduction roasting at a set temperature in a rotary kiln and then cooled to obtain direct reduced iron.
[0009] Optionally, the metallurgical dust includes: one or more of LT fine ash, sewage sedimentation sludge, ironmaking dry process ash, gas ash, and LT coarse ash, and the metallurgical dust is pretreated to obtain the raw material, including:
[0010] LT fine ash, sewage sedimentation sludge, ironmaking dry process ash, gas ash and LT coarse ash are respectively subjected to dust and sludge wetting and homogenization treatment, and then mixed to obtain raw materials.
[0011] Optionally, in the raw materials, by mass fraction, the sum of the contents of LT fine ash and LT coarse ash is 40% to 50%, the content of gas ash is 35% to 40%, the content of ironmaking dry process ash is 8% to 11%, and the content of sewage sludge is 2% to 10%.
[0012] Optionally, the set mass ratio of the raw materials to the auxiliary materials and the fuel is (85-88):(1-2):(10-13).
[0013] Optionally, the auxiliary material includes limestone.
[0014] Optionally, the fuel comprises coke powder.
[0015] Optionally, the alkalinity of the mixture is 1.75 to 1.95.
[0016] Optionally, the set temperature of the reduction roasting is 1050°C to 1150°C.
[0017] In a second aspect, the present application provides a direct reduced iron prepared by the method described in any one of the embodiments of the second aspect, wherein the metallization rate of the direct reduced iron is ≥75%.
[0018] Optionally, in the direct reduced iron, the content of TFe is 50% to 60%, and the content of MFe is 40% to 50%, calculated by mass fraction.
[0019] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0020] The present application provides a method for preparing direct reduced iron using metallurgical dust, comprising: pre-treating the metallurgical dust to obtain raw materials; mixing the raw materials with auxiliary materials and fuel according to a set mass ratio to obtain a mixture; in terms of mass fraction, in the mixture, the content of TFe is 34% to 38%, and the content of C is 20% to 30%; the mixture is subjected to reduction roasting at a set temperature in a rotary kiln, and then cooled to obtain direct reduced iron. By controlling the content of various metallurgical dusts in the raw materials, as well as the mass ratio of the raw materials to the auxiliary materials and fuel, the ratio of C / Fe in the mixture is regulated, which is conducive to the reduction reaction. In addition, while utilizing the metallurgical dust, the recovery rate of the iron-containing material in the metallurgical dust is improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0022] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0023] Figure 1 A schematic flow chart of a method for preparing direct reduced iron using metallurgical dust and sludge provided in an embodiment of the present application. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0025] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0026] In addition, in the description of the specification of the present application, the terms "including", "comprising", etc. mean "including but not limited to". In this article, relational terms such as "first" and "second", etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A and B can be singular or plural. In this article, "at least one" means one or more, and "plurality" means two or more. "At least one", "the following at least one item (items)" or similar expressions refer to any combination of these items, including any combination of single items (items) or plural items (items). For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or plural, respectively.
[0027] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0028] The production of direct reduced iron from metallurgical dust is a process in which metallurgical dust is mixed and formed at a certain temperature, and the iron oxide in the dust is reduced to metallic iron under the action of a reducing agent. Direct reduced iron has the advantages of stable chemical composition, low impurity content, and low cost of use. Therefore, it can be used as a raw material for electric furnace steelmaking, as a coolant for converter steelmaking, and can also replace part of sintered ore as a charge for blast furnace ironmaking.
[0029] The rotary kiln is a relatively traditional process for producing direct reduced iron and solid waste treatment. At present, there are quite a few rotary kilns used to treat zinc-containing solid waste, but most of them do not belong to steel companies. They are mainly used to treat other high-zinc-containing solid wastes in society and high-zinc-containing solid wastes in steel companies. The medium and low zinc-containing solid wastes of steel companies have not been fully utilized, and these treatment equipment are relatively backward. Some are directly transformed from eliminated cement kilns, with low environmental protection levels, which limits the development of rotary kilns.
[0030] However, the present invention aims to recover iron-containing materials in metallurgical dust to the maximum extent. At the same time, considering that the rotary kiln process is shorter than that of the rotary hearth furnace and does not require agglomeration, as long as the unorganized emissions of the raw material processing system are effectively controlled and the carbon contained in the solid waste is fully utilized, coke powder is used as a supplementary reducing agent and heat supplement. It has the advantages of low investment and operating costs, iron-rich materials can be used for sintering, blast furnaces, converters, etc. after screening, and no secondary pollution of solid waste will be generated. Therefore, a method for producing direct reduced iron from metallurgical dust using a rotary kiln process is provided.
[0031] Figure 1 A schematic flow chart of a method for preparing direct reduced iron using metallurgical dust and sludge provided in an embodiment of the present application.
[0032] See also Figure 1 The present application provides a method for preparing direct reduced iron using metallurgical dust and mud, the method comprising:
[0033] S1, pre-treating metallurgical dust and mud to obtain raw materials;
[0034] In some embodiments, the metallurgical dust includes: one or more of LT fine ash, sewage sedimentation sludge, ironmaking dry process ash, gas ash, and LT coarse ash, and the metallurgical dust is pretreated to obtain the raw material, including:
[0035] LT fine ash, sewage sedimentation sludge, ironmaking dry process ash, gas ash and LT coarse ash are respectively subjected to dust and sludge wetting and homogenization treatment, and then mixed to obtain raw materials.
[0036] In some embodiments, in the raw material, the sum of the contents of LT fine ash and LT coarse ash is 40% to 50%, the content of gas ash is 35% to 40%, the content of ironmaking dry process ash is 8% to 11%, and the content of sewage sludge is 2% to 10%, calculated by mass fraction.
[0037] It should be noted that the primary dust removal of the converter adopts a dry method (LT), the ash coming out of the evaporative cooler is coarse ash, and the ash coming out of the electrostatic precipitator is fine ash, thereby distinguishing LT fine ash and LT coarse ash. By controlling the content of various metallurgical dust muds in the raw materials, the ratio of C / Fe in the mixture is regulated, which is conducive to the reduction reaction. Exemplarily, in terms of mass fraction, in the raw materials, the sum of the content of LT fine ash and LT coarse ash can be 40%, 42%, 44%, 46%, 48%, 50%, etc., the content of gas ash is 35%, 36%, 37%, 38%, 39%, 40%, etc., the content of ironmaking dry ash can be 8%, 9%, 10%, 11%, etc., and the content of sewage sedimentation sludge can be 2%, 3%, 4%, 6%, 8%, 10%, etc.
[0038] S2. Mixing the raw material, auxiliary material and fuel according to a set mass ratio to obtain a mixture; in the mixture, the content of TFe is 34% to 38%, and the content of C is 20% to 30% by mass fraction;
[0039] In some embodiments, the set mass ratio of the raw material to the auxiliary material and the fuel is (85-88):(1-2):(10-13).
[0040] It should be noted that the set mass ratio of raw materials to auxiliary materials and fuel is raw materials: auxiliary materials: fuel = (85-88): (1-2): (10-13). The reason for adopting this ratio in the mixture is to adjust the C / Fe ratio, which is conducive to the occurrence of the reduction reaction. Exemplarily, the set mass ratio can be 85:2:13, 86:2:12, 87:2:11, 88:2:10, 86:1:13, 88:1:11, etc.
[0041] In some embodiments, the auxiliary material includes limestone.
[0042] In some embodiments, the fuel includes coke fines.
[0043] In some embodiments, the alkalinity of the mixture is 1.75-1.95.
[0044] By adding limestone, the basicity of the mixture is adjusted, and coke powder is added as a supplementary reducing agent and a heat supplement. At the same time, by controlling the content of various metallurgical dusts in the raw materials, as well as the mass ratio of the raw materials to the auxiliary materials and the fuel, the ratio of C / Fe in the mixture is regulated, which is beneficial to the reduction reaction. Exemplarily, the basicity of the mixture can be 1.75, 1.80, 1.85, 1.90, 1.95, etc. In terms of mass fraction, in the mixture, the content of TFe can be 34%, 35%, 36%, 37%, 38%, etc., and the content of C can be 20%, 22%, 24%, 26%, 28%, 30%, etc.
[0045] S3, reducing and roasting the mixed material at a set temperature in a rotary kiln, and then cooling the mixed material to obtain direct reduced iron.
[0046] In some embodiments, the reduction roasting is set at a temperature of 1050°C to 1150°C.
[0047] The reduction reaction is promoted by high temperature roasting. Within this temperature range, the metallization rate of the kiln slag and the recovery rate of zinc powder after reduction can meet the requirements. For example, the set temperature of the reduction roasting can be 1050°C, 1080°C, 1100°C, 1120°C, 1150°C, etc.
[0048] Based on a general inventive concept, the present application provides a direct reduced iron, wherein the metallization rate of the direct reduced iron is ≥75%.
[0049] In some embodiments, in the direct reduced iron, the content of TFe is 50% to 60%, and the content of MFe is 40% to 50%, calculated by mass fraction.
[0050] The direct reduced iron (metallized kiln slag) prepared by the present application can be used as high-quality raw and auxiliary materials for steelmaking. The present application makes comprehensive use of the metallurgical dust and mud resources produced by steel enterprises, and produces direct reduced iron with a high metallization rate, which has very significant economic and environmental benefits. Exemplarily, the metallization rate of the direct reduced iron can be 75%, 76%, 77%, 78%, 80%, 82%, etc. In the direct reduced iron, the content of TFe can be 50%, 52%, 54%, 56%, 58%, 60%, etc., and the content of MFe can be 40%, 42%, 44%, 46%, 48%, 50%, etc.
[0051] The direct reduced iron is realized based on the preparation method of the direct reduced iron mentioned above. The specific steps of the preparation method of the direct reduced iron can refer to the above embodiment. Since the direct reduced iron adopts part or all of the technical solutions of the above embodiment, it has at least all the beneficial effects brought by the technical solutions of the above embodiment, which will not be described one by one here.
[0052] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to industry standards. If there is no corresponding industry standard, then the conditions recommended by the manufacturer are followed.
[0053] Example 1
[0054] This embodiment provides a method for preparing direct reduced iron using metallurgical dust and mud, the method comprising the following steps:
[0055] S11. LT fine ash, LT coarse ash, gas ash, dry process ash and sewage sedimentation sludge are mixed in a ratio of 45:5:38:10:2 to obtain a raw material.
[0056] S21. The raw material, limestone powder and coke powder are mixed in a ratio of 86:2:12 to obtain a mixture, wherein the TFe content of the mixture is 34.76% and the C content is 21.4%.
[0057] S31, the mixed material is evenly added into the rotary kiln from the top of the kiln tail, and is spirally transported to the kiln head in the rotary kiln. After preheating, drying, heating, and reduction roasting stages, hot kiln slag is obtained. The temperature of the rotary kiln reduction roasting stage is 1060℃.
[0058] S41, cooling the hot slag obtained in step S31 to obtain direct reduced iron.
[0059] Example 2
[0060] This embodiment provides a method for preparing direct reduced iron using metallurgical dust and mud, the method comprising the following steps:
[0061] S11. LT fine ash, LT coarse ash, gas ash, dry process ash and sewage sedimentation sludge are mixed in a ratio of 48:2:38:8:4 to obtain a raw material.
[0062] S21. The raw material, limestone powder and coke powder are mixed in a ratio of 88:1:11 to obtain a mixture, wherein the TFe content of the mixture is 36.66% and the C content is 23.60%.
[0063] S31, the mixed material is evenly added into the rotary kiln from the top of the kiln tail, and is spirally transported to the kiln head in the rotary kiln. After preheating, drying, heating, and reduction roasting stages, hot kiln slag is obtained. The temperature of the rotary kiln reduction roasting stage is 1120℃.
[0064] S41, cooling the hot slag obtained in step S31 to obtain direct reduced iron.
[0065] Example 3
[0066] This embodiment provides a method for preparing direct reduced iron using metallurgical dust and mud, the method comprising the following steps:
[0067] S11. LT fine ash, LT coarse ash, gas ash, dry process ash and sewage sedimentation sludge are mixed in a ratio of 40:10:36:8:6 to obtain a raw material.
[0068] S21. The raw material, limestone powder and coke powder are mixed in a ratio of 87:1:12 to obtain a mixture, wherein the TFe content of the mixture is 38.95% and the C content is 23.6%.
[0069] S31, the mixed material is evenly added into the rotary kiln from the top of the kiln tail, and is spirally transported to the kiln head in the rotary kiln. After preheating, drying, heating, and reduction roasting stages, hot kiln slag is obtained. The temperature of the rotary kiln reduction roasting stage is 1100℃.
[0070] S41, cooling the hot slag obtained in step S31 to obtain direct reduced iron.
[0071] Example 4
[0072] This embodiment provides a method for preparing direct reduced iron using metallurgical dust and mud, the method comprising the following steps:
[0073] S11. LT fine ash, LT coarse ash, gas ash, dry process ash and sewage sludge are mixed in a ratio of 42:5:40:8:5 to obtain a raw material.
[0074] S21. The raw material, limestone powder and coke powder are mixed in a ratio of 86:1:13 to obtain a mixture, wherein the TFe content of the mixture is 35.87% and the C content is 25.08%.
[0075] S31. The mixed material is evenly added into the rotary kiln from the top of the kiln tail and is spirally transported to the kiln head in the rotary kiln. After preheating, drying, heating, and reduction roasting stages, hot kiln slag is obtained. The temperature of the rotary kiln reduction roasting stage is 1150℃.
[0076] S41, cooling the hot slag obtained in step S31 to obtain direct reduced iron.
[0077] Comparative Example 1
[0078] This comparative example provides a method for preparing direct reduced iron using metallurgical dust and mud, the method comprising the following steps:
[0079] S11. LT fine ash, LT coarse ash, gas ash, dry process ash and sewage sludge are mixed in a ratio of 30:20:10:20:20 to obtain a raw material.
[0080] S21. The raw material, limestone powder and coke powder are mixed in a ratio of 86:2:12 to obtain a mixture, wherein the TFe content of the mixture is 31.53% and the C content is 17.4%.
[0081] S31, the mixed material is evenly added into the rotary kiln from the top of the kiln tail, and is spirally transported to the kiln head in the rotary kiln. After preheating, drying, heating, and reduction roasting stages, hot kiln slag is obtained. The temperature of the rotary kiln reduction roasting stage is 1080℃.
[0082] S41, cooling the hot slag obtained in step S31 to obtain direct reduced iron.
[0083] Comparative Example 2
[0084] This comparative example provides a method for preparing direct reduced iron using metallurgical dust and mud, the method comprising the following steps:
[0085] S11. LT fine ash, LT coarse ash, gas ash, dry process ash and sewage sedimentation sludge are mixed in a ratio of 43:5:40:8:4 to obtain a raw material.
[0086] S21. The raw material, limestone powder and coke powder are mixed in a ratio of 93:2:5 to obtain a mixture, wherein the TFe content of the mixture is 35.76% and the C content is 15.4%.
[0087] S31, the mixed material is evenly added into the rotary kiln from the top of the kiln tail, and is spirally transported to the kiln head in the rotary kiln. After preheating, drying, heating, and reduction roasting stages, hot kiln slag is obtained. The temperature of the rotary kiln reduction roasting stage is 1100℃.
[0088] S41, cooling the hot slag obtained in step S31 to obtain direct reduced iron.
[0089] Comparative Example 3
[0090] This comparative example provides a method for preparing direct reduced iron using metallurgical dust and mud, the method comprising the following steps:
[0091] S11. LT fine ash, LT coarse ash, gas ash, dry process ash and sewage sedimentation sludge are mixed in a ratio of 40:7:39:11:3 to obtain a raw material.
[0092] S21. The raw material, limestone powder and coke powder are mixed in a ratio of 93:2:5 to obtain a mixture, wherein the TFe content of the mixture is 37.26% and the C content is 22.5%.
[0093] S31, the mixed material is evenly added into the rotary kiln from the top of the kiln tail, and is spirally transported to the kiln head in the rotary kiln. After preheating, drying, heating, and reduction roasting stages, hot kiln slag is obtained. The temperature of the rotary kiln reduction roasting stage is 900℃.
[0094] S41, cooling the hot slag obtained in step S31 to obtain direct reduced iron.
[0095] The direct reduced iron obtained in Examples 1 to 4 and Comparative Examples 1 to 3 was tested for TFe and MFe and the metallization rate was calculated, and the results are shown in Table 1.
[0096] Table 1 TFe, MFe content (wt, %) and metallization rate of direct reduced iron
[0097] Group TFe% MFe% Metallization rate % Example 1 54.63 41.82 76.55 Example 2 57.23 42.96 75.07 Example 3 56.99 43.71 76.70 Example 4 54.27 43.00 79.14 Comparative Example 1 53.28 35.64 66.89 Comparative Example 2 56.32 32.56 57.81 Comparative Example 3 55.27 34.32 62.10
[0098] As shown in Table 1, the metallization rates of the direct reduced iron obtained in Comparative Examples 1 to 3 are only 66.89%, 57.81% and 62.10% respectively, while the metallization rates of the direct reduced iron obtained in Examples 1 to 4 by using the method of the present invention are all over 75%, which is 9% to 20% higher than that in the comparative examples. This indicates that by using the technical solution of the present invention, the metallurgical dust and mud resources generated by the steel enterprises are comprehensively utilized, and the direct reduced iron with a high metallization rate is produced, which has very significant economic and environmental benefits.
[0099] In addition, one or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:
[0100] In the embodiment of the present invention, the proportion of C in the mixture and the temperature of the rotary kiln reduction roasting stage are controlled, so that the reducing agent is used to reduce the substances such as zinc ferrite mainly present in the metallurgical dust at high temperature to reduce them into zinc vapor, which is then oxidized to be recovered as secondary zinc oxide, thereby improving the recovery rate of zinc powder.
[0101] In the embodiments of the present invention, the purpose is to remove zinc and recover iron-containing materials in metallurgical dust to the maximum extent. At the same time, considering that the rotary kiln process is shorter than that of the rotary hearth furnace and does not require agglomeration, as long as the unorganized emissions of the raw material processing system are effectively controlled and the carbon contained in the solid waste is fully utilized, coke powder is used as a supplementary reducing agent and heat supplement, which has the advantages of low investment and operating costs, iron-rich materials can be used for sintering, blast furnaces, converters, etc. after screening, and no secondary pollution of solid waste will be generated.
[0102] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for preparing direct reduced iron using metallurgical dust and sludge, characterized in that: The method comprises: Pre-treating metallurgical dust and mud to obtain raw materials; The raw material, auxiliary material and fuel are mixed according to a set mass ratio to obtain a mixture; in the mixture, the content of TFe is 34% to 38%, and the content of C is 20% to 30% by mass fraction; The mixed material is subjected to reduction roasting at a set temperature in a rotary kiln and then cooled to obtain direct reduced iron.
2. The method according to claim 1, characterized in that The metallurgical dust includes: one or more of LT fine ash, sewage sedimentation sludge, ironmaking dry process ash, gas ash, and LT coarse ash. The metallurgical dust is pretreated to obtain the raw material, including: LT fine ash, sewage sedimentation sludge, ironmaking dry process ash, gas ash and LT coarse ash are respectively subjected to dust and sludge wetting and homogenization treatment, and then mixed to obtain raw materials.
3. The method according to claim 2, characterized in that In terms of mass fraction, in the raw materials, the sum of LT fine ash and LT coarse ash is 40% to 50%, the content of gas ash is 35% to 40%, the content of ironmaking dry process ash is 8% to 11%, and the content of sewage sedimentation sludge is 2% to 10%.
4. The method according to claim 1, characterized in that The set mass ratio of the raw materials to the auxiliary materials and the fuel is (85-88):(1-2):(10-13).
5. The method according to claim 4, characterized in that The auxiliary material includes limestone.
6. The method according to claim 4, characterized in that The fuel includes coke powder.
7. The method according to claim 1, characterized in that The basicity of the mixture is 1.75-1.
95.
8. The method according to claim 1, characterized in that The set temperature of the reduction roasting is 1050°C to 1150°C.
9. Direct reduced iron prepared by the method according to any one of claims 1 to 8, characterized in that: The metallization rate of the direct reduced iron is ≥75%.
10. The direct reduced iron according to claim 9, characterized in that: In terms of mass fraction, in the direct reduced iron, the content of TFe is 50% to 60%, and the content of MFe is 40% to 50%.
Citation Information
Patent Citations
Method for removing alkali metal in metallurgical dust mud
CN106480310A
Method for treating metallurgical dust and sludge
CN108728636A
Method for improving strength of iron-rich kiln slag of rotary kiln
CN114075622A
Method for making steel by directly utilizing iron-rich kiln slag of rotary kiln
CN114891997A
Modification sintering treatment method for waste dust and sludge of steel mill
CN115725835A
Cited By
Process method for treating alumina red mud by using rotary cement kiln
CN122076799A