Magnesium-based composite material deep-cavity cylindrical casting and preparation method and application thereof

By using specific proportions of raw materials and low-pressure casting technology in magnesium-based composite materials, combined with stress annealing and solid solution treatment, the problems of molding defects and insufficient mechanical properties of deep cavity cylindrical castings of magnesium-based composite materials have been solved, and the problem of insufficient mechanical properties of magnesium-based composite materials has been significantly improved. Forming capability and mechanical properties.

CN118910440APending Publication Date: 2024-11-08SHAANXI UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410717199.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The deep-cavity cylindrical castings of magnesium-based composite materials are prone to introduce casting defects during the molding process, which affects their mechanical properties. Especially under harsh heavy load conditions, it is difficult for the prior art to effectively improve their forming ability and mechanical properties.

Method used

Pure Mg ingots, pure Zn ingots, Mg-Gd intermediate alloy, Mg-Y intermediate alloy, Mg-Zr intermediate alloy and SiC solid particles were melted, cast under a filling pressure of 0.1 to 0.15MPa, and then stress annealing , uniform solid solution and aging treatment to optimize the microstructure and mechanical properties of magnesium-based composite materials.

Benefits of technology

The tensile strength, yield strength and elongation of deep-cavity cylindrical castings of magnesium-based composite materials have been improved, ensuring the improvement of its forming ability and mechanical properties. The tensile strength reaches 320~340MPa, the yield strength is 240~260MPa, and the elongation is It is 3% to 4%, and the modulus is 68GPa.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910440A_ABST
    Figure CN118910440A_ABST
Patent Text Reader

Abstract

The invention discloses a magnesium-based composite material deep-cavity cylindrical casting and a preparation method and application thereof, and belongs to the technical field of casting. The preparation method comprises the following steps: weighing a pure Mg ingot, a pure Zn ingot, an Mg-Gd intermediate alloy, an Mg-Y intermediate alloy, an Mg-Zr intermediate alloy and SiC solid particles, smelting, heating to 750-780 DEG C, casting under the mold filling pressure of 0.1-0.15 MPa, and carrying out stress annealing treatment, homogenization solid solution treatment and aging treatment to obtain the magnesium-based composite material deep-cavity cylindrical casting with excellent performance. The preparation method is simple, rapid and efficient, the prepared magnesium-based composite material deep-cavity cylindrical casting is complete in mold filling and uniform in texture and has excellent formability and mechanical property, the tensile strength is 320-340 MPa, the yield strength is 240-260 MPa, the ductility is 3%-4%, and the modulus is 68 GPa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of casting, and in particular relates to a magnesium-based composite material deep-cavity cylindrical casting and a preparation method and application thereof. Background Art

[0002] As the lightest nonferrous metal in structural engineering applications, magnesium has a very important significance and huge application potential in the lightweight process of aerospace, automobiles and combat weapons. Although magnesium and magnesium alloys are the preferred materials for lightweighting, the mechanical properties of magnesium alloys are not excellent under harsh heavy load conditions. The design and creation of magnesium-based composite materials provide development conditions for the emergence of high-strength and high-modulus magnesium alloys. Magnesium-based composite materials are made by adding various non-metallic materials, such as ceramics or carbon materials, to magnesium or magnesium alloys in order to empower the natural intrinsic advantages of the strengthening phase and enhance the structural properties of magnesium alloys.

[0003] At present, magnesium-based composite materials can indeed greatly improve the strength and modulus of magnesium alloys while maintaining the lightweight advantages of magnesium alloys. However, with the addition of SiC particles, the viscosity of the composite melt increases significantly, and the convective heat transfer of the melt in the crucible is weakened during the smelting process, causing the inhomogeneity of the melt temperature field to increase, directly affecting the formability of complex castings. At the same time, due to the large gap in the thermophysical properties of magnesium alloys and inorganic ceramic particles, magnesium-based composite materials are prone to casting defects during the molding process of complex castings, thereby affecting the mechanical properties of complex components of magnesium-based composite materials.

[0004] The molding of deep-cavity cylindrical parts has always been a difficult point in magnesium alloy casting. Deep-cavity cylindrical parts often have different solidification rates at different parts of the casting due to the excessive depth of the cylinder wall, which introduces a large number of casting defects and affects the forming ability and mechanical properties of the cylindrical parts. Summary of the invention

[0005] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a magnesium-based composite material deep-cavity cylindrical casting and a preparation method and application thereof, so as to solve the technical problem of low forming ability and mechanical properties of magnesium-based composite material deep-cavity cylindrical casting.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] The first aspect of the present invention discloses a method for preparing a deep-cavity cylindrical casting of a magnesium-based composite material, comprising weighing pure Mg ingots, pure Zn ingots, Mg-Gd master alloys, Mg-Y master alloys, Mg-Zr master alloys and SiC solid particles for smelting, heating to 750-780° C., and casting at a filling pressure of 0.1-0.15 MPa to obtain a deep-cavity cylindrical casting of a magnesium-based composite material;

[0008] Among them, the Mg content is 88.3wt.%, the Zn content is 0.2wt.%, the Gd content is 8wt.%, the Y content is 3.1wt.%, the Zr content is 0.4wt.%, and the added amount of SiC particles is 14wt.% of the total amount of pure Mg ingot, pure Zn ingot and Mg intermediate alloy.

[0009] Preferably, the smelting step is: weigh a pure Mg ingot and completely melt it, then add a pure Zn ingot, Mg-Gd master alloy, Mg-Y master alloy and Mg-Zr master alloy and stir at 760°C, and add SiC solid particles while stirring for smelting.

[0010] Preferably, before smelting, the SiC solid particles are preheated at 500° C. for not less than 30 minutes.

[0011] Preferably, after the temperature is raised to 750-780° C., a scum removal treatment is performed on the surface of the mixed raw material.

[0012] Preferably, during the entire smelting process, a protective gas consisting of CO2 and SF6 in a ratio of 40:1 is continuously introduced.

[0013] Preferably, the specific steps of casting are: pouring the smelted mixed raw materials into a mold, maintaining the pressure at a filling pressure of 0.1 to 0.15 MPa and a hydraulic speed of 3 mm / s for 5 to 10 minutes, and demolding.

[0014] Preferably, the mold is a bottom pouring mold with a circular gate cross section.

[0015] Preferably, after casting, stress annealing treatment, homogenization solid solution treatment and aging treatment are performed to obtain a deep-cavity cylindrical casting of a magnesium-based composite material.

[0016] Further preferably, the step of stress annealing treatment is: heating the cast magnesium-based composite material raw material to 220° C. at 220° C. / 1 h, keeping the temperature, and cooling along with the furnace.

[0017] Preferably, the steps of homogenizing solid solution and aging treatment are: subjecting the magnesium-based composite material raw material after stress annealing to solid solution treatment at 480°C / 24h, furnace cooling, and then subjecting it to aging treatment at 225°C / 36h.

[0018] The second aspect of the present invention discloses a magnesium-based composite material deep-cavity cylindrical casting obtained by the above-mentioned preparation method.

[0019] Preferably, the magnesium-based composite material deep-cavity cylindrical casting has a tensile strength of 320-340 MPa, a yield strength of 240-260 MPa, and an elongation of 3%-4%.

[0020] The third aspect of the present invention discloses the use of the above-mentioned magnesium-based composite material deep-cavity cylindrical casting in the preparation of aerospace parts or automobile parts.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The present invention provides a method for preparing a deep-cavity cylindrical casting of a magnesium-based composite material, 1) using pure Mg ingots, pure Zn ingots, Mg-Gd master alloys, Mg-Y master alloys, Mg-Zr master alloys and SiC solid particles as smelting raw materials, Zn can improve the structure of magnesium, improve the strength and hardness of the alloy, improve the corrosion resistance of the deep-cavity cylindrical casting, and improve the processing performance of the deep-cavity cylindrical casting; Gd can improve the strength and hardness of the deep-cavity cylindrical casting, and improve the thermal stability and high-temperature resistance of the deep-cavity cylindrical casting; Zr can improve the strength and plasticity of the deep-cavity cylindrical casting, improve the structure of the magnesium alloy, and improve the heat resistance of the deep-cavity cylindrical casting; Y can improve the strength and hardness of the deep-cavity cylindrical casting, and improve the corrosion resistance and heat resistance of the deep-cavity cylindrical casting. 2) Adding SiC particles on the basis of the above raw materials can effectively refine the grains and improve the texture, thereby improving the mechanical properties of the magnesium alloy. 3) The use of specific proportions of each component of the mixed raw material can better utilize the promoting effect of each metal element on the alloy and further improve the performance of the magnesium alloy. 4) The low-pressure casting method of 0.1-0.15MPa is adopted, so that the magnesium-based composite material mixed slurry can be filled evenly, smoothly and completely, which can give the product a denser structure and ensure that the mechanical properties of the deep-cavity cylindrical parts meet the requirements through stress relief annealing to ensure the performance and quality of the magnesium-based composite material deep-cavity cylindrical castings. Therefore, the preparation method is simple, fast and efficient, and the obtained magnesium-based composite material deep-cavity cylindrical castings are completely filled, uniform in texture, and have excellent formability and mechanical properties, with a tensile strength of 320-340MPa, a yield strength of 240-260MPa, an elongation of 3%-4%, and a modulus of 68GPa.

[0023] Furthermore, preheating the SiC particles before adding them can ensure that when the SiC particles are added to the composite material molten metal, defects such as poor bonding and holes will not occur due to a large temperature difference between the two.

[0024] Furthermore, since magnesium easily reacts chemically with oxygen to generate oxide impurities, a protective gas composed of CO2 and SF6 in a volume ratio of 40:1 is continuously introduced during the smelting process to isolate oxygen.

[0025] Furthermore, the gate cross-section of the bottom pouring casting mold is circular, and the circular cross-section can improve the shrinkage compensation efficiency.

[0026] Furthermore, the strength of the obtained deep-cavity cylindrical casting can be further improved through stress annealing, homogenization solution and aging treatment. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The three-dimensional model diagram of the present invention; wherein, (a) mold model; (b) casting model; (c) mold cross-sectional view;

[0028] Figure 2 This is a macroscopic image of a casting obtained in Example 1 of the present invention;

[0029] Figure 3 The metallographic structure diagram of the casting obtained in Example 1 of the present invention;

[0030] Figure 4 This is a SEM image of the casting obtained in Example 1 of the present invention;

[0031] Figure 5 It is a schematic diagram of the structure of the tensile specimen used in the tensile test;

[0032] Figure 6 The figure is a comparison chart of the mechanical properties of the castings obtained in Example 1 and Example 2 of the present invention. DETAILED DESCRIPTION

[0033] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.

[0034] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.

[0035] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values ​​within the range (including integers and fractions).

[0036] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.

[0037] In this paper, the melting temperature of the magnesium ingot is 720°C, the addition temperature of the master alloy is 760°C, the semi-solid temperature range of the melt is 615°C, and the casting temperature is 750-780°C.

[0038] The present invention provides a method for preparing a deep-cavity cylindrical casting of a magnesium-based composite material, comprising the following steps:

[0039] Step 1: Raw material preparation

[0040] The raw materials required for the matrix alloy of the magnesium-based composite material are weighed according to the weight ratio: pure Mg ingot, pure Zn ingot, Mg master alloy and SiC solid particles;

[0041] The content of Mg is 88.3wt.%, and the content of Zn is 0.2wt.%; the Mg master alloy includes Mg-Gd master alloy, Mg-Y master alloy and Mg-Zr master alloy, and the content of Gd in the Mg master alloy is 8wt.%, the content of Y is 3.1wt.%, and the content of Zr is 0.4wt.%. The amount of SiC particles added is 14wt.% of the total amount of pure Mg ingot, pure Zn ingot and Mg master alloy.

[0042] Step 2: Melting

[0043] The weighed pure Mg ingot is placed in a smelting container and heated to 720°C. After the pure Mg ingot is completely melted, the temperature is continued to be raised to 760°C. Then the weighed pure Zn ingot, Mg-Gd master alloy, Mg-Y master alloy and Mg-Zr master alloy are added. The mixture is stirred at a low speed of 90 to 110 rpm without eddy current for 10 to 12 minutes. After the alloy components are fully mixed, a composite material molten metal is obtained.

[0044] Preheat the weighed SiC particles at 500°C for not less than 30 min.

[0045] The temperature of the composite material molten metal is lowered to 615°C, and then stirred at a speed of 1150-1250rpm / min for 18-20min. During the stirring period, under the action of the vortex flow on the surface of the composite material molten metal, the preheated SiC particles are quickly added to make the SiC particles evenly dispersed in the composite material molten metal to obtain a magnesium-based composite material mixed slurry. The magnesium-based composite material mixed slurry is heated to 750-780°C, and the surface of the magnesium-based composite material mixed slurry is subjected to a scum removal treatment.

[0046] During the entire smelting process, a protective gas consisting of CO2 and SF6 with a volume ratio of 40:1 is continuously introduced.

[0047] Step 3: Low pressure casting

[0048] The bottom pouring mold was preheated to 560°C, then placed on a 380t hydraulic press, and a lubricant consisting of graphite and oil was applied to the inner wall of the mold.

[0049] The magnesium-based composite material mixed mud which has been removed of the scum and heated to 750-780°C is poured into the preheated bottom-injection casting mold. After the magnesium-based composite material mixed mud is completely poured in, the pressure head is placed at the main flow channel, and the hydraulic press is controlled to maintain the pressure at a filling pressure of 0.1-0.15MPa and a hydraulic speed of 3mm / s for 5-10min until the magnesium-based composite material mixed mud is completely filled in the mold cavity. Then the hydraulic press returns, the pressure head is taken out, and the mold temperature is cooled to 200-250°C, and the cylindrical part is demolded;

[0050] The bottom pouring casting mold has four evenly distributed gates, and the gate cross-section is circular.

[0051] Step 4: Stress annealing

[0052] The cylindrical part after demoulding in the third step is heated to 220°C at 220°C / 1h, kept warm, and then gradually cooled slowly along with the furnace;

[0053] Here, 220°C / 1h means heat treatment at 220°C for 1 hour.

[0054] Step 5: Homogenization solution / aging treatment

[0055] The cylindrical part after cooling in the fourth step is subjected to solution treatment at 480°C / 24h, furnace cooling at room temperature, and then aging treatment at 225°C / 36h to obtain a magnesium-based composite material deep cavity cylindrical casting, such as Figure 1 shown.

[0056] The magnesium-based composite material deep-cavity cylindrical component has a tensile strength of 320-340 MPa, a yield strength of 240-260 MPa, an elongation of 3%-4%, and a modulus of 68 GPa.

[0057] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0058] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, and ratio means weight ratio.

[0059] Example 1

[0060] A method for preparing a deep-cavity cylindrical casting of a magnesium-based composite material, the preparation method is as follows:

[0061] Accurately weigh 4.525 kg of pure Mg, 1.963 kg of Mg-30Gd alloy, 0.761 kg of Mg-30Y alloy, 0.098 kg of Mg-30Zr alloy and 0.015 kg of pure Zn ingot.

[0062] The weighed pure Mg ingot was placed in a stainless steel crucible in the furnace of a resistance furnace, and a 40:1 ratio of CO2 mixed with SF6 was continuously introduced into the stainless steel crucible as a protective gas. When the temperature of the resistance furnace was raised to 720°C, the magnesium ingot was completely melted, and the temperature was further raised to 760°C. Pure Zn ingots, Mg-30Gd master alloy, Mg-30Y master alloy and Mg-30Zr master alloy (where 30 represents the mass fraction) were added to the stainless steel crucible in sequence, and then stirred at 100 rpm without eddy current for 10 minutes. After the alloy components were fully mixed, a composite metal liquid was obtained.

[0063] The weighed SiC particles were preheated at 500°C for 30 min.

[0064] The temperature of the composite material molten metal is lowered to 615°C, and then the preheated SiC particles are quickly added while stirring at a speed of 1200 rpm / min, so that the SiC particles are evenly dispersed in the composite material molten metal to obtain a magnesium-based composite material mixed slurry. The magnesium-based composite material mixed slurry is then heated to 770°C, and then the surface of the magnesium-based composite material mixed slurry is treated to remove scum.

[0065] The bottom-injection casting mold with a circular gate cross-section was preheated to 560°C, then placed on a 380t hydraulic press, and a lubricant consisting of graphite and oil was applied to the inner wall of the mold.

[0066] The mixed slurry with the scum removed and heated to 770℃ is poured into the preheated mold. After the melt is completely poured in, the pressure head is placed at the main channel. At this time, the hydraulic press moves downward at a uniform speed with a filling pressure of 0.1MPa and a hydraulic rate of 3mm / s until the melt completely fills the mold cavity. The holding time is controlled at 10min. Then the hydraulic press returns, the pressure head is taken out, and the mold temperature is cooled to 200℃, the cylindrical part is demolded, and then heated to 220℃ at 220℃ / 1h, kept warm, and gradually cooled slowly with the furnace. After that, the solution treatment is carried out at 480℃ / 24h, and the furnace is cooled at room temperature, and then the aging treatment is carried out at 225℃ / 36h to obtain the Mg-8.0Gd-3.1Y-0.4Zr-0.2Zn deep cavity cylindrical casting.

[0067] like Figure 2 As shown, the casting has a smooth appearance, a complete structure, and no obvious defects are found, indicating that the casting result is ideal. Figure 3 Metallographic diagram and Figure 4 The SEM images show that the grain size is very uniform, the SiC particles are also evenly distributed, and there is no obvious particle agglomeration phenomenon, indicating that the mechanical properties of the deep cavity cylindrical castings are improved.

[0068] Example 2

[0069] A method for preparing a deep-cavity cylindrical casting of a magnesium-based composite material, the preparation method is as follows:

[0070] Accurately weigh 4.525 kg of pure Mg ingot, 1.963 kg of Mg-30Gd alloy, 0.761 kg of Mg-30Y alloy, 0.098 kg of Mg-30Zr alloy and 0.015 kg of pure Zn ingot.

[0071] The weighed pure Mg ingot was placed in a stainless steel crucible in the furnace of a resistance furnace, and a 40:1 ratio of CO2 mixed with SF6 was continuously introduced into the stainless steel crucible as a protective gas. When the temperature of the resistance furnace was raised to 720°C, the magnesium ingot was completely melted, and the temperature was further raised to 760°C. Pure Zn ingots, Mg-30Gd master alloy, Mg-30Y master alloy and Mg-30Zr master alloy (where 30 represents the mass fraction) were added to the stainless steel crucible in sequence, and then stirred at 100rpm without eddy current for 10 minutes. After the alloy components were fully mixed, a composite material metal liquid was obtained.

[0072] The weighed SiC particles were preheated at 500°C for 30 min.

[0073] The temperature of the composite material molten metal is lowered to 615°C, and then the preheated SiC particles are quickly added while stirring at a speed of 1200 rpm / min, so that the SiC particles are evenly dispersed in the composite material molten metal to obtain a magnesium-based composite material mixed slurry. Subsequently, the magnesium-based composite material mixed slurry is heated to 750°C, and then the surface of the magnesium-based composite material mixed slurry is treated to remove scum.

[0074] The bottom-injection casting mold with a circular gate cross-section was preheated to 560°C, then placed on a 380t hydraulic press, and a lubricant consisting of graphite and oil was applied to the inner wall of the mold.

[0075] The mixed slurry with the scum removed and heated to 750℃ is poured into the preheated mold. After the melt is completely poured in, the pressure head is placed at the main channel. At this time, the hydraulic press moves downward at a uniform speed with a filling pressure of 0.15MPa and a hydraulic rate of 3mm / s until the melt completely fills the mold cavity. The holding time is controlled at 10min. Then the hydraulic press returns, the pressure head is taken out, and the mold temperature is cooled to 200℃, the cylindrical part is demolded, and then heated to 220℃ at 220℃ / 1h, kept warm, and gradually cooled slowly with the furnace. After that, the solution treatment is carried out at 480℃ / 24h, and the furnace is cooled at room temperature, and then the aging treatment is carried out at 225℃ / 36h to obtain the Mg-8.0Gd-3.1Y-0.4Zr-0.2Zn deep cavity cylindrical casting.

[0076] To investigate the mechanical properties of the deep-cavity cylindrical casting of the magnesium-based composite material prepared by the above method, the steps are as follows: tensile specimens ( Figure 5 ), a tensile test machine was used to carry out a tensile test to detect the corresponding elongation, yield strength and tensile strength.

[0077] The experimental results are as follows Figure 6 As shown, the tensile strength of the magnesium-based composite material tensile specimen obtained in Example 1 is 337MPa, the yield strength is 250.8MPa, the elongation is 3.6%, and the modulus is 68GPa. The tensile strength of the magnesium-based composite material tensile specimen obtained in Example 2 is 334MPa, the yield strength is 243MPa, the elongation is 3.8%, and the modulus is 68GPa. The results show that the forming ability and mechanical properties of the deep-cavity cylindrical castings obtained by this method are improved, and the better casting scheme is a casting temperature of 770°C, a mold preheating temperature of 560°C, and a filling pressure of 0.1MPa.

[0078] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A method for preparing a deep-cavity cylindrical casting of a magnesium-based composite material, characterized in that: Weigh pure Mg ingots, pure Zn ingots, Mg-Gd master alloys, Mg-Y master alloys, Mg-Zr master alloys and SiC solid particles for smelting, heat to 750-780° C., and cast at a filling pressure of 0.1-0.15 MPa to obtain a deep-cavity cylindrical casting of a magnesium-based composite material; Among them, the Mg content is 88.3wt.%, the Zn content is 0.2wt.%, the Gd content is 8wt.%, the Y content is 3.1wt.%, the Zr content is 0.4wt.%, and the added amount of SiC particles is 14wt.% of the total amount of pure Mg ingot, pure Zn ingot and Mg intermediate alloy.

2. The method for preparing a deep cavity cylindrical casting of a magnesium-based composite material according to claim 1, characterized in that: The smelting steps are: weigh pure Mg ingots and completely melt them, then add pure Zn ingots, Mg-Gd master alloy, Mg-Y master alloy and Mg-Zr master alloy and stir at 760°C, and add SiC solid particles for smelting while stirring.

3. The method for preparing a deep cavity cylindrical casting of a magnesium-based composite material according to claim 1, characterized in that: Before smelting, the SiC solid particles are preheated at 500°C for not less than 30 minutes.

4. The method for preparing a deep cavity cylindrical casting of a magnesium-based composite material according to claim 1, characterized in that: After the temperature is raised to 750-780°C, the surface of the mixed raw material is treated to remove scum.

5. The method for preparing a deep cavity cylindrical casting of a magnesium-based composite material according to claim 1, characterized in that: During the entire smelting process, a protective gas consisting of CO2 and SF6 in a ratio of 40:1 is continuously introduced.

6. The method for preparing a deep cavity cylindrical casting of a magnesium-based composite material according to claim 1, characterized in that: The specific steps of casting are: pouring the smelted mixed raw materials into the mold, maintaining the pressure for 5 to 10 minutes at a filling pressure of 0.1 to 0.15 MPa and a hydraulic speed of 3 mm / s, and demolding.

7. A method for preparing a magnesium-based composite material deep cavity cylindrical casting according to any one of claims 1 to 6, characterized in that: After casting, stress annealing, homogenization and solid solution treatment and aging treatment are performed to obtain a deep-cavity cylindrical casting of a magnesium-based composite material.

8. A magnesium-based composite material deep-cavity cylindrical casting obtained by the preparation method according to any one of claims 1 to 7.

9. The deep cavity cylindrical casting of magnesium-based composite material according to claim 8, characterized in that: The tensile strength of the deep-cavity cylindrical casting of the magnesium-based composite material is 320-340 MPa, the yield strength is 240-260 MPa, and the elongation is 3%-4%.

10. Use of the deep-cavity cylindrical casting of magnesium-based composite material according to claim 8 or 9 in the preparation of aerospace parts or automobile parts.