Aluminum foil, aluminum foil preparation method, pole piece and battery
By adding rare earth elements and B elements to the aluminum foil and using electromagnetic stirring and refining agent to the aluminum foil, the problem of low elongation of alloy aluminum foil is solved, the purity and elongation of the aluminum foil are improved, and the overall performance and safety of the battery are improved. .
Patent Information
- Application Number
- CN202410871877.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-06-28
AI Technical Summary
The elongation of alloy aluminum foil is low, which affects the deformation ability of the battery during charging and discharging, and thus affects the overall performance and safety of the battery.
By adding rare earth elements such as La, Ce, Pr, Tb and Yb to the aluminum foil, combining elements B, and using electromagnetic stirring and refining agent to treat, the purity and grain structure of the aluminum alloy liquid are improved, and high-purity aluminum foil is formed and the growth of the large amount of aluminum foil is increased. Elongation and tensile strength.
It improves the purity and elongation of the aluminum foil, improves the overall performance and safety of the battery, and ensures the good deformation ability of the aluminum foil in the battery.
Smart Images

Figure CN118910472A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of foil materials. Specifically, the present application relates to an aluminum foil, an aluminum foil preparation method, an electrode sheet and a battery. Background Art
[0002] Alloy aluminum foil is a common material for battery current collectors, with excellent conductivity and stability. However, due to the low elongation of alloy aluminum foil, the current collector has insufficient deformation ability during battery charging and discharging, which in turn affects the overall performance and safety of the battery. Summary of the invention
[0003] One purpose of the embodiments of the present application is to provide a new technical solution for aluminum foil, aluminum foil preparation method, pole piece and battery.
[0004] According to a first aspect of an embodiment of the present application, an aluminum foil is provided, comprising the following components by mass percentage:
[0005] Fe: 0.15-0.20%, Si: 0.05-0.10%, Cu: 0.02-0.05%; Ti: 0.01-0.03%, rare earth elements: 0.02-0.2%, the balance is Al and unavoidable impurities;
[0006] The rare earth element includes at least one of La, Ce, Pr, Tb and Yb.
[0007] Optionally, the rare earth element includes La.
[0008] Optionally, the rare earth elements include La and Ce.
[0009] Optionally, the rare earth elements include La, Ce and Pr.
[0010] Optionally, the rare earth elements include La, Ce, Pr and Tb.
[0011] Optionally, the rare earth elements include La, Ce, Pr, Tb and Yb.
[0012] Optionally, the mass ratio of La to Ce is (0.5-2):1.
[0013] Optionally, the aluminum foil further contains B, and the content of B is 0.01%-0.05%.
[0014] Optionally, the tensile strength of the aluminum foil is in the range of 200 MPa-220 MPa, and the elongation of the aluminum foil is greater than or equal to 4.0%.
[0015] According to a second aspect of an embodiment of the present application, a method for preparing an aluminum foil is provided, comprising:
[0016] Smelting aluminum-containing raw materials, iron-containing raw materials, silicon-containing raw materials, copper-containing raw materials, titanium-containing raw materials and optional rare earth raw materials to obtain a first aluminum alloy liquid;
[0017] adding a refiner to the first aluminum alloy liquid to perform a refinement treatment to obtain a second aluminum alloy liquid;
[0018] The second aluminum alloy liquid is subjected to cold rolling and annealing treatment and then foil rolling to obtain the aluminum foil described in the first aspect.
[0019] Optionally, the smelting treatment conditions include electromagnetic stirring, the temperature of the electromagnetic stirring is 450° C.-750° C., and the time of the electromagnetic stirring is 40 min-70 min.
[0020] Optionally, the electromagnetic stirring comprises:
[0021] The first aluminum alloy liquid is subjected to first-stage stirring, wherein the first-stage stirring temperature is 450° C.-550° C., and the first-stage stirring time is 3-5 min;
[0022] The first aluminum alloy liquid is subjected to second-stage stirring, wherein the second-stage stirring temperature is 550° C.-650° C., and the second-stage stirring time is 8-10 min;
[0023] The first aluminum alloy liquid is subjected to a third stage of stirring, wherein the temperature of the third stage of stirring is 650° C.-750° C., and the time of the third stage of stirring is 10-20 min;
[0024] The first aluminum alloy liquid is subjected to fourth stage stirring, the temperature of the fourth stage stirring is 650° C.-750° C., and the time of the third stage stirring is 20-30 minutes.
[0025] Optionally, the refiner includes at least one of Al-Ti-B-rare earth, LaB6 and Al-Ti-BC-rare earth.
[0026] According to a third aspect of an embodiment of the present application, a pole piece is provided, the pole piece comprising a current collector and an active material, wherein the active material is coated on at least one side surface of the current collector;
[0027] The current collector adopts the aluminum foil described in the first aspect.
[0028] According to a fourth aspect of an embodiment of the present application, a battery is provided, comprising the pole piece described in the third aspect.
[0029] A technical effect of this application is:
[0030] An embodiment of the present application provides an aluminum foil, which includes the following components, by mass percentage: Fe: 0.15-0.20%, Si: 0.05-0.10%, Cu: 0.02-0.05%; Ti: 0.01-0.03%, rare earth elements: 0.02-0.2%, and the remainder is Al and unavoidable impurities; wherein the rare earth elements include at least one of La, Ce, Pr, Tb and Yb, which is beneficial to improving the purity of the aluminum foil, reducing the enrichment of impurity elements in the aluminum foil, and improving the elongation of the aluminum foil.
[0031] Other features and advantages of the present application will become apparent from the following detailed description of exemplary embodiments of the present application with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] The accompanying drawings, which are incorporated in and constitute a part of the specification, illustrate embodiments of the application and, together with the description, serve to explain the principles of the application.
[0033] Figure 1 A schematic diagram of a pole piece provided for one embodiment of the present application. DETAILED DESCRIPTION
[0034] Various exemplary embodiments of the present application will now be described in detail with reference to the accompanying drawings. It should be noted that unless otherwise specifically stated, the relative arrangement of components and steps, numerical expressions and numerical values set forth in these embodiments do not limit the scope of the present application.
[0035] The embodiments of the present application will be described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and should not be understood as limiting the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.
[0036] The term "first" or "second" in the specification and claims of this application may include one or more of the features explicitly or implicitly. In the description of this application, unless otherwise specified, "plurality" means two or more. In addition, "and / or" in the specification and claims means at least one of the connected objects, and the character " / " generally means that the objects connected before and after are in an "or" relationship.
[0037] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0038] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0039] It should be noted that like reference numerals and letters refer to similar items in the following figures, and therefore, once an item is defined in one figure, it need not be further discussed in subsequent figures.
[0040] The present application embodiment provides an aluminum foil, which comprises the following components by mass percentage:
[0041] Fe (iron): 0.15-0.20%, Si (silicon): 0.05-0.10%, Cu (copper): 0.02-0.05%; Ti (titanium): 0.01-0.03%, rare earth elements: 0.02-0.2%, the balance is Al (aluminum) and unavoidable impurities;
[0042] The rare earth element includes at least one of La (lanthanum), Ce (cerium), Pr (praseodymium), Tb (terbium) and Yb (ytterbium).
[0043] In this embodiment, the raw material of the aluminum foil may be a high-purity aluminum alloy doped with rare earth elements. The high-purity aluminum alloy may be 1060 aluminum alloy or 1080 aluminum alloy to reduce the contents of components such as Fe, Si and Cu in the aluminum alloy.
[0044] Specifically, Fe, Si and Cu easily form compounds with aluminum, and these compounds are insoluble in the aluminum alloy solution and exist in the aluminum alloy solution as a second phase, which easily reduces the purity and quality of the aluminum foil; and during the rolling process of the aluminum foil, the enrichment of Fe and Si will lead to more impurities in the aluminum foil, thereby affecting the physical properties of the aluminum foil such as purity and electrical conductivity.
[0045] The aluminum foil provided in the embodiment of the present application has a higher purity of aluminum alloy, so that the content of impurities such as Fe, Si, Cu and Ti is lower, which is beneficial to improving the purity of the aluminum foil, reducing the enrichment of impurity elements in the aluminum foil, and is beneficial to improving the elongation of the aluminum foil, enhancing the deformation ability of the aluminum foil, and ensuring the overall performance and safety of the battery using the aluminum foil.
[0046] In this embodiment, the contents of impurities such as Mn, Mg and Zn are even lower, for example, by mass percentage, Mn: 0.02-0.03%, Mg: <0.01%, Zn: <0.01%, which can ensure the purity of the aluminum foil after forming.
[0047] The aluminum foil provided in the embodiment of the present application includes the following components: Fe: 0.15-0.20%, Si: 0.05-0.10%, Cu: 0.02-0.05%; Ti: 0.01-0.03%, rare earth elements: 0.02-0.2%, and the balance is Al and unavoidable impurities; wherein the rare earth elements include at least one of La, Ce, Pr, Tb and Yb, which is beneficial to improving the purity of the aluminum foil, reducing the enrichment of impurity elements in the aluminum foil, and improving the elongation of the aluminum foil.
[0048] In one embodiment, the rare earth element includes La.
[0049] In this embodiment, when La is added to the aluminum foil, it can act as a nucleation center in the aluminum foil. At the same time, La can produce LaB compounds to homogenize the grain structure. Moreover, during the casting and rolling process of the aluminum foil, La can improve the internal structure of the aluminum foil and enhance the structural stability of the aluminum foil.
[0050] In one embodiment, the rare earth elements include La and Ce.
[0051] In this embodiment, on the basis of La element improving the internal structure of the aluminum foil, Ce element can promote the formation of Al cubic texture in the aluminum foil. The cubic texture can increase the specific surface area of the aluminum foil and enhance the electrical conductivity of the aluminum foil.
[0052] In one embodiment, the rare earth elements include La, Ce, and Pr.
[0053] In this embodiment, on the basis that La element improves the internal structure of aluminum foil and Ce element increases the specific surface area of aluminum foil, Pr element can refine the grains of aluminum foil, and such grain refinement helps to improve the mechanical properties of aluminum alloy, so that the aluminum foil has higher strength and better toughness.
[0054] In one embodiment, the rare earth elements include La, Ce, Pr and Tb.
[0055] In this embodiment, on the basis that the la element improves the internal structure of the aluminum foil, the Ce element increases the specific surface area of the aluminum foil, and the Pr element improves the strength and toughness of the aluminum foil, the Tb element can promote the formation of compounds in the aluminum foil and change the microstructure of the alloy, thereby improving the corrosion resistance of the aluminum foil.
[0056] In one embodiment, the rare earth elements include La, Ce, Pr, Tb and Yb.
[0057] In this embodiment, on the basis of the la element improving the internal structure of the aluminum foil, the Ce element increasing the specific surface area of the aluminum foil, the Pr element improving the strength and toughness of the aluminum foil, and the Tb element improving the corrosion resistance of the aluminum foil, the Yb element can further improve the hardness and strength of the alloy, improve the microstructure and mechanical properties of the aluminum foil, and increase the corrosion resistance of the aluminum foil.
[0058] In one embodiment, the mass ratio of La to Ce is (0.5-2):1.
[0059] In this embodiment, the aluminum foil includes, by mass percentage:
[0060] La: 0.01-0.1%; Ce: 0.01-0.1%.
[0061] Since La can act as the nucleation center in aluminum foil and produce LaB compounds, it can homogenize the grain structure. Moreover, during the casting and rolling process of aluminum foil, La can improve the internal structure of the aluminum foil and improve the structural stability of the aluminum foil. The Ce element can cooperate with La to promote the formation of Al cubic texture in the aluminum foil. The cubic texture can increase the specific surface area of the aluminum foil and increase the electrical conductivity of the aluminum foil.
[0062] In one embodiment, the aluminum foil further contains B (boron), and the content of B is 0.01%-0.05%.
[0063] In this embodiment, element B is added to the aluminum foil in the form of a refiner. Element B forms compounds with Ti and rare earth elements in the aluminum foil, which can act as a nucleation center and refine the grains of the aluminum foil during casting and rolling, so that the aluminum foil has higher strength and better toughness.
[0064] In one embodiment, the tensile strength of the aluminum foil is in the range of 200-220 MPa, and the elongation of the aluminum foil is greater than or equal to 4.0%.
[0065] Adding rare earth elements to the aluminum alloy solution can form smaller and more evenly distributed grains, while reducing the generation and growth of the second phase, making the aluminum grain structure finer and more uniform, thereby effectively increasing the elongation of the aluminum foil without reducing the strength of the aluminum foil.
[0066] The present application also provides a method for preparing an aluminum foil, the method comprising:
[0067] S101, smelting an aluminum-containing raw material, an iron-containing raw material, a silicon-containing raw material, a copper-containing raw material, a titanium-containing raw material and an optional rare earth raw material to obtain a first aluminum alloy liquid;
[0068] S102, adding a refiner to the first aluminum alloy liquid to perform a refinement treatment to obtain a second aluminum alloy liquid;
[0069] S103, subjecting the second aluminum alloy liquid to cold rolling and annealing treatments and then to foil rolling to obtain the above-mentioned aluminum foil.
[0070] In this embodiment, the forming raw material of the aluminum foil includes an aluminum alloy and a refiner, the refiner includes a refinement component and a rare earth element component, and the rare earth element component includes at least one of La, Ce, Pr, Tb and Yb.
[0071] During the aluminum foil forming process, refiners can be added to the molten aluminum alloy solution. The refinement components can promote the formation of crystal nuclei in the aluminum alloy, refine large grains into small particle sizes, and help improve the microstructure of the aluminum alloy, thereby improving the strength and elongation of the aluminum foil.
[0072] In one embodiment, adding a refiner to the first aluminum alloy liquid for refinement may include adding a refiner containing a rare earth raw material to the first aluminum alloy liquid being smelted for refinement, or adding a refiner containing a rare earth raw material to the first aluminum alloy liquid after smelting for refinement. The refiner containing a rare earth raw material may be at least one of Al-Ti-B-rare earth, LaB6, and Al-Ti-BC-rare earth.
[0073] In one embodiment, the aluminum foil provided in the embodiment of the present application is doped with rare earth elements in a refiner after smelting, and the refinement component and the rare earth element component are added to the liquid aluminum alloy solution in the form of a refiner, which can significantly reduce the hydrogen content in the aluminum alloy solution, reduce the porosity and impurity elements of the aluminum foil, thereby improving the purity and deformation quality of the aluminum foil.
[0074] In one embodiment, the Si content in the refiner is less than 0.10%, the Fe content is less than 0.15%, the Ti content is in the range of 4.4-4.6%, the rare earth element content is in the range of 0.8-1.2%, the B content is in the range of 0.7-1%, and the Al content is in the range of 94-96%.
[0075] In one embodiment, the smelting treatment conditions include electromagnetic stirring, the temperature of the electromagnetic stirring is 450° C.-750° C., and the time of the electromagnetic stirring is 40 min-70 min.
[0076] During the aluminum foil forming process, the refiner is added into the aluminum alloy solution in the form of filaments, and the aluminum alloy solution is electromagnetically stirred.
[0077] When the refiner is added to the aluminum alloy solution in the form of filaments, electromagnetic stirring of the aluminum alloy solution can make the rare earth elements in the refiner better absorbed by the elements in the aluminum alloy and make the rare earth elements more evenly distributed in the aluminum foil.
[0078] Specifically, after the aluminum alloy solution is electromagnetically stirred, the aluminum alloy solution also needs to undergo the processes of casting, cold rolling and foil rolling. The rare earth elements are better absorbed by the elements in the aluminum alloy, which can reduce the contact between the rare earth elements and the rolling elements during casting, cold rolling and foil rolling, thereby avoiding the formation of large-grained second phase structure during cold rolling and foil rolling, and ensuring the purity of the aluminum foil.
[0079] In one embodiment, the electromagnetic stirring comprises:
[0080] The first aluminum alloy liquid is subjected to first-stage stirring, wherein the first-stage stirring temperature is 450° C.-550° C., and the first-stage stirring time is 3-5 min;
[0081] The first aluminum alloy liquid is subjected to second-stage stirring, wherein the second-stage stirring temperature is 550° C.-650° C., and the second-stage stirring time is 8-10 min;
[0082] The first aluminum alloy liquid is subjected to a third stage of stirring, wherein the temperature of the third stage of stirring is 650° C.-750° C., and the time of the third stage of stirring is 10-20 min;
[0083] The first aluminum alloy liquid is subjected to fourth stage stirring, the temperature of the fourth stage stirring is 650° C.-750° C., and the time of the third stage stirring is 20-30 minutes.
[0084] In a specific embodiment, the electromagnetic stirring comprises:
[0085] When one third of the first aluminum alloy liquid is melted, the first aluminum alloy liquid is stirred in the first stage, the stirring temperature in the first stage is 450° C.-550° C., and the stirring time in the first stage is 3-5 min;
[0086] When the first aluminum alloy liquid is half melted, the first aluminum alloy liquid is stirred in the second stage, the stirring temperature in the second stage is 550° C.-650° C., and the stirring time in the second stage is 8-10 minutes;
[0087] When the first aluminum alloy liquid is three-quarters melted, the first aluminum alloy liquid is stirred in the third stage, the stirring temperature in the third stage is 650° C.-750° C., and the stirring time in the third stage is 10-20 min;
[0088] After the first aluminum alloy liquid is completely melted, the first aluminum alloy liquid is subjected to fourth stage stirring, the stirring temperature of the fourth stage is 650° C.-750° C., and the stirring time of the third stage is 20-30 min.
[0089] In this embodiment, the electromagnetic stirring includes first stage stirring, second stage stirring, third stage stirring and fourth stage stirring;
[0090] When the aluminum alloy is one third melted, the molten aluminum alloy is stirred in the first stage;
[0091] When the aluminum alloy is half melted, the molten aluminum alloy is stirred in the second stage;
[0092] When two-thirds of the aluminum alloy is melted, the molten aluminum alloy is stirred in the first stage;
[0093] When the aluminum alloy is completely melted, the molten aluminum alloy is subjected to a fourth stage of stirring.
[0094] In this embodiment, when the molten aluminum alloy is stirred in the first stage, the refiner has been added to the aluminum alloy. The first stage stirring, the second stage stirring, and the third stage stirring can fully melt the aluminum alloy ingot, and filter the gas in the aluminum alloy solution through stirring, and remove the excess oxygen and carbon components in the aluminum alloy solution, so as to achieve the purpose of purifying the aluminum solution and ensure the purity of the aluminum foil after forming.
[0095] The fourth stage of stirring can be carried out at a temperature of about 700°C. At this time, the aluminum alloy has been completely melted into a solution, and the rare earth elements can react with the aluminum alloy elements to form intermetallic compounds.
[0096] After electromagnetic stirring, the forming process also includes casting, cold rolling, intermediate annealing, cold rolling and foil rolling. The above-mentioned intermetallic compounds can be dispersedly distributed on the grain boundaries in the aluminum foil during the cooling process. The hardness of the intermetallic compounds is relatively low and they are easily destroyed during the cold rolling process. The destroyed intermetallic compounds containing rare earth elements play a role in inhibiting grain growth after intermediate annealing, and can refine the grains before foil rolling. Therefore, during the foil rolling process, the deformation of each part of the aluminum foil is uniform through uniform grain distribution, which improves the yield rate of aluminum foil obtained by foil rolling. Moreover, at this time, Fe and Si are rarely aggregated due to the reaction of rare earth elements, and the probability of second phase aggregation in the aluminum foil is greatly reduced, which can ensure the elongation of the aluminum foil.
[0097] In this embodiment, rare earth elements are doped into a refiner after smelting. Adding the rare earth elements into the liquid aluminum alloy solution in the form of a refiner can significantly reduce the hydrogen content in the aluminum alloy solution, reduce the porosity and impurity elements of the aluminum foil, and thus improve the purity and deformation quality of the aluminum foil.
[0098] In this embodiment, when the molten aluminum alloy is stirred in the first stage, the stirring temperature is 450°C-550°C, and the stirring time is 3-5 minutes. At this stage, the refiner has been added to the aluminum alloy to avoid the refiner from melting too quickly at high temperature. The first stage stirring, the second stage stirring, and the third stage stirring are continuously heated within the temperature range of 450°C-750°C, so that the aluminum alloy ingot can be fully melted, and the gas in the aluminum alloy solution is filtered by stirring, and the excess oxygen and carbon components in the aluminum alloy solution are removed at the same time, so as to achieve the purpose of purifying the aluminum solution and ensure the purity of the aluminum foil after forming.
[0099] The fourth stage stirring can be carried out at a temperature of 650°C-750°C. For example, the fourth stage stirring is carried out at a temperature of 700°C. At this time, the aluminum alloy has been completely melted into a solution, and the rare earth elements can react with the aluminum alloy elements to form intermetallic compounds.
[0100] In a specific embodiment, the method for preparing aluminum foil comprises the following steps:
[0101] S201, adding an aluminum alloy ingot into a smelting furnace, the initial temperature of the smelting furnace is 770-800°C, the aluminum alloy ingot is partially melted and then kept warm for 10 minutes, and then cooled to 700-750°C along with the smelting furnace;
[0102] S202, controlling the temperature of the aluminum alloy solution at 700-750° C., adding the above-mentioned refiner into the aluminum flow trough in the form of filaments, the diameter of the filaments being 8-10 mm, and the adding speed being 1-1.5 kg / min;
[0103] S203, when the aluminum alloy ingot is melted to one-third liquid, the first stage of stirring can be carried out, and the stirring time is 5 minutes; when the aluminum alloy ingot is melted to half, the second stage of stirring can be carried out, and the stirring time is 8-10 minutes; when the aluminum alloy ingot is melted to three-quarters, the third stage of stirring can be carried out, and the stirring time is not more than 10 minutes; after the aluminum alloy ingot is completely melted, the fourth stage of stirring is carried out during the process of adding the refiner, and the stirring time is not more than 30 minutes, and the stirring frequency is 20-40Hz;
[0104] S204, allowing the stirred solution to stand for 6-20 minutes at a standing furnace temperature of 700-750° C., and then starting casting and rolling at a casting and rolling speed of 900-1100 mm / min. The thickness of the cast-rolled aluminum plate after casting and rolling is 6.5-8 mm;
[0105] S205, the first cold rolling, the first cold rolling adopts two passes, the first pass reduction is about 50%, the aluminum plate thickness is 3-4mm, the second pass reduction is 40-49%, the aluminum plate thickness is about 2mm;
[0106] S206, intermediate annealing, the intermediate annealing temperature is 200-450℃, and the annealing time is 30-40min;
[0107] S207, the second cold rolling, the second cold rolling is three passes, the reduction of each pass is maintained at 50%-60%, the thickness after the first rolling is rolled from 2mm to 0.8-0.9mm, the thickness after the second rolling is 0.4-0.45mm, and the thickness after the third rolling is 0.2-0.22mm. At this time, the aluminum billet is a foil rolling raw material billet;
[0108] S208, the foil billet with a thickness of 0.2-0.22mm is subjected to four passes of foil rolling, the first pass is rough rolling, the middle two passes are medium rolling, and the last pass is finish rolling. The thickness after the first pass is 90-100μm, the thickness after the second pass is 40-50μm, the thickness after the third pass is 20-25μm, and the aluminum foil with a thickness of 13μm is obtained after the last pass.
[0109] In one embodiment, the refiner includes at least one of Al-Ti-B-rare earth, LaB6, and Al-Ti-BC-rare earth.
[0110] In this embodiment, taking La and Ce rare earth elements as an example, La and Ce rare earth elements are added to the aluminum alloy solution in the form of refiners, which can not only reduce the introduction of impurity elements in the process, but also La and Ce in the rare earth elements can improve the distribution and size of TiB2, making TiB2 particles smaller and more uniform; in the formed aluminum foil, La and Ce elements can act as the nucleation center of the grain together with the refinement components to refine the size of the grain and reduce the growth of the La and Ce second phases.
[0111] Specifically, La and Ce directly affect the grain size and distribution of titanium boride and titanium aluminide in the refiner. The titanium boride and titanium aluminide in the refiner usually exist as a second phase, which acts as a nucleation center in the aluminum alloy solution. However, the size of the second phase is relatively large, usually around 30 μm. The addition of La and Ce rare earth elements can improve the activity energy of titanium and boron particles, reduce the aggregation of titanium boride and titanium aluminide, and make the titanium boride and titanium aluminide particles dispersed in the aluminum foil matrix, thereby enhancing the refinement effect of the refiner.
[0112] In one embodiment, in Al-Ti-B, the mass ratio of Ti to B is in the range of (3.5-5.5):1, which ensures sufficient TiB2 particle formation and achieves effective grain refinement.
[0113] See also Figure 1 , an embodiment of the present application provides a pole piece, the pole piece comprising a current collector 1 and an active material 2, wherein the active material 2 is coated on at least one side surface of the current collector 1;
[0114] The current collector 1 is made of the above-mentioned aluminum foil.
[0115] In this embodiment, the purity of the aluminum alloy in the above-mentioned aluminum foil is high, so that the content of impurities such as Fe, Si, Cu and Ti is lower, which is beneficial to improving the purity of the aluminum foil, reducing the enrichment of impurity elements in the aluminum foil, and is beneficial to improving the elongation of the aluminum foil, enhancing the deformation ability of the aluminum foil, and ensuring the overall performance and safety of the battery using the aluminum foil.
[0116] An embodiment of the present application provides a battery, which includes the pole piece described above.
[0117] In this embodiment, the battery includes a positive electrode sheet, a separator and a negative electrode sheet. The separator is arranged between the positive electrode sheet and the negative electrode sheet. The positive electrode collector in the positive electrode sheet adopts the above-mentioned aluminum foil. The elongation of the aluminum foil is improved, thereby ensuring the overall performance and safety of the battery.
[0118] The aluminum foil of the present application is described in detail below using examples and comparative examples.
[0119] The mass percentage (wt %) and mass ratio of each element in each embodiment and comparative example are shown in Table 1.
[0120] Table 1 Mass percentage (wt%) and mass ratio of each element
[0121]
[0122]
[0123]
[0124] The aluminum foil obtained from the above examples and comparative examples was tested:
[0125] Specifically, the aluminum foil was subjected to a tensile test using the specimens and methods for tensile testing of deformed aluminum, magnesium and alloy products in GB / T 16865-2013. The aluminum foil tensile specimen was 150 mm long and 15 mm wide, and the gauge length was 50 mm.
[0126] Table 2 Test results of tensile strength and elongation of aluminum foil
[0127]
[0128]
[0129] It can be seen from the test in Table 2 that high-purity aluminum alloy is used in Examples 1 to 19, and rare earth elements are added, so that the tensile strength of the aluminum foil is above 200 MPa and the elongation reaches above 4.1%, ensuring the deformation ability of the aluminum foil.
[0130] Compared with Example 1, the mass percentage of some component elements in Comparative Examples 1 to Comparative Examples 10 is too low or too high, resulting in the tensile strength of the aluminum foil being lower than 200 MPa and the elongation being lower than 3.8%, which limits the deformation capacity of the aluminum foil.
[0131] The following examples and comparative examples are used to explain in detail the method for preparing the aluminum foil of the present application.
[0132] Embodiment 101
[0133] (1) adding aluminum-containing raw materials, iron-containing raw materials, silicon-containing raw materials, copper-containing raw materials, titanium-containing raw materials and rare earth raw materials into a smelting furnace, the initial temperature of the smelting furnace is 780° C., the aluminum alloy ingot is melted and kept warm for 10 minutes, and then cooled to 735° C. with the furnace;
[0134] (2) When the aluminum alloy solution temperature is 735°C, the refiner (Al-Ti-B-rare earth) is added into the aluminum flow trough in the form of filaments with a diameter of 9.5 mm and an addition rate of 1.2 kg / min;
[0135] (3) cold rolling the refiner and the aluminum alloy solution to obtain an aluminum billet having a thickness of 0.21 mm;
[0136] (4) Annealing the aluminum billet at a temperature of 300° C. for 25 min;
[0137] (5) The annealed aluminum material is subjected to foil rolling to obtain an aluminum foil with a thickness of 13 μm. The aluminum foil comprises: Fe: 0.16%, Si: 0.06%, Cu: 0.03%; Ti: 0.02%, La: 0.02%, Ce: 0.02%, and the remainder is aluminum and unavoidable impurities.
[0138] Embodiment 102
[0139] Electromagnetic stirring is used before cold rolling the refiner and the aluminum alloy solution, and the other steps are the same as Example 101.
[0140] The temperature of electromagnetic stirring was 700°C and the time was 60 min.
[0141] Embodiment 103
[0142] Electromagnetic stirring is used before cold rolling the refiner and the aluminum alloy solution, and the other steps are the same as Example 101.
[0143] The temperature of electromagnetic stirring was 450°C and the time was 41 min.
[0144] Embodiment 104
[0145] Electromagnetic stirring is used before cold rolling the refiner and the aluminum alloy solution, and the other steps are the same as Example 101.
[0146] The temperature of electromagnetic stirring was 750°C and the time was 65 min.
[0147] Embodiment 105
[0148] Before cold rolling the refiner and the aluminum alloy solution, staged electromagnetic stirring is used, and the other steps are the same as Example 101.
[0149] The stirring temperature in the first stage is 500°C, and the stirring time in the first stage is 4 minutes;
[0150] The stirring temperature of the second stage is 600°C, and the stirring time of the second stage is 8 minutes;
[0151] The stirring temperature in the third stage is 700°C, and the stirring time in the third stage is 15 minutes;
[0152] The stirring temperature in the fourth stage is 700° C., and the stirring time in the third stage is 25 min.
[0153] Embodiment 106
[0154] Al-Ti-B refiner is selected to replace Al-Ti-B-rare earth refiner, and the other steps are the same as Example 101.
[0155] Table 3 Test results of tensile strength and elongation of aluminum foil
[0156] example tensile strength Elongation Embodiment 101 206 4.2 Embodiment 102 208 4.4 Embodiment 103 209 4.6 Embodiment 104 211 4.5 Embodiment 105 206 4.5 Embodiment 106 206 4.0
[0157] It can be seen from the test in Table 3 that, compared with Example 106, Example 101 uses a refiner containing rare earth elements added to the molten aluminum alloy solution, which can improve the strength and elongation of the aluminum foil.
[0158] In Examples 102 to 105, electromagnetic stirring of the aluminum alloy solution can enable the rare earth elements in the refiner to be better absorbed by the elements in the aluminum alloy and make the rare earth elements more evenly distributed in the aluminum foil, thereby ensuring the purity and elongation of the aluminum foil.
[0159] Although some specific embodiments of the present application have been described in detail by way of example, it should be understood by those skilled in the art that the above examples are only for illustration, not for limiting the scope of the present application. It should be understood by those skilled in the art that the above embodiments may be modified without departing from the scope and spirit of the present application. The scope of the present application is defined by the appended claims.
Claims
1. An aluminum foil, characterized in that: Calculated by mass percentage, it includes the following components: Fe: 0.15%-0.20%, Si: 0.05%-0.10%, Cu: 0.02%-0.05%; Ti: 0.01%-0.03%, rare earth elements: 0.02-0.2%, the balance is Al and unavoidable impurities; Wherein, the rare earth element includes at least one of La, Ce, Pr, Tb and Yb.
2. The aluminum foil according to claim 1, characterized in that The rare earth element includes La.
3. The aluminum foil according to claim 1, characterized in that The rare earth elements include La and Ce.
4. The aluminum foil according to claim 1, characterized in that The rare earth elements include La, Ce and Pr.
5. The aluminum foil according to claim 1, characterized in that The rare earth elements include La, Ce, Pr and Tb.
6. The aluminum foil according to claim 1, characterized in that The rare earth elements include La, Ce, Pr, Tb and Yb.
7. The aluminum foil according to claim 3, characterized in that The mass ratio of La to Ce is (0.5-2):
1.
8. The aluminum foil according to claim 1, characterized in that The aluminum foil also contains B, and the content of B is 0.01%-0.05%.
9. The aluminum foil according to claim 1, characterized in that The tensile strength of the aluminum foil is in the range of 200 MPa-220 MPa, and the elongation of the aluminum foil is greater than or equal to 4.0%.
10. A method for preparing aluminum foil, characterized in that: include: Smelting aluminum-containing raw materials, iron-containing raw materials, silicon-containing raw materials, copper-containing raw materials, titanium-containing raw materials and optional rare earth raw materials to obtain a first aluminum alloy liquid; adding a refiner to the first aluminum alloy liquid to perform a refinement treatment to obtain a second aluminum alloy liquid; The second aluminum alloy liquid is subjected to cold rolling and annealing treatment and then foil rolling to obtain the aluminum foil as claimed in any one of claims 1 to 9.
11. The preparation method according to claim 10, characterized in that: The smelting treatment conditions include electromagnetic stirring, the temperature of the electromagnetic stirring is 450° C.-750° C., and the time of the electromagnetic stirring is 40 min-70 min.
12. The preparation method according to claim 11, characterized in that: The electromagnetic stirring comprises: The first aluminum alloy liquid is subjected to first-stage stirring, wherein the first-stage stirring temperature is 450° C.-550° C., and the first-stage stirring time is 3-5 min; The first aluminum alloy liquid is subjected to second-stage stirring, wherein the second-stage stirring temperature is 550° C.-650° C., and the second-stage stirring time is 8-10 min; The first aluminum alloy liquid is subjected to a third stage of stirring, wherein the temperature of the third stage of stirring is 650° C.-750° C., and the time of the third stage of stirring is 10-20 min; The first aluminum alloy liquid is subjected to fourth stage stirring, the temperature of the fourth stage stirring is 650° C.-750° C., and the time of the third stage stirring is 20-30 minutes.
13. The preparation method according to claim 10, characterized in that: The refiner includes at least one of Al-Ti-B-rare earth, LaB6 and Al-Ti-BC-rare earth.
14. A pole piece, characterized in that: It comprises a current collector (1) and an active material (2), wherein the active material (2) is coated on at least one side surface of the current collector (1); The current collector (1) is made of the aluminum foil described in any one of claims 1 to 9.
15. A battery, characterized in that: Including the pole piece as claimed in claim 14.
Citation Information
Patent Citations
Special rare earth-containing aluminum alloy foil for pole tab and preparation method of special rare earth-containing aluminum alloy foil
CN103436746A
Preparation method of aluminum foil current collector for lithium ion power battery
CN108630944A
0.008-0.016 mm H18 specification lithium battery current collector aluminum foil and production process thereof
CN116043071A
Preparation method of SiC nano-particle reinforced aluminum alloy
CN116656993A
Aluminum foil and its production
JP1997272938A
Cited By
High-extension aluminum foil for battery positive electrode and production method thereof
CN120924842A
A high-ductility aluminum foil for battery positive electrode and its production method
CN120924842B