Composite coating and application thereof in improving wettability of liquid metal to surface of solid matrix

By setting a composite coating structure with a high thermal conductivity intermediate layer and an infiltration layer on the solid surface, the problem of poor wetting of liquid metal on the solid surface is solved, and large-area spread of liquid metal on the solid surface is achieved and high-efficiency heat dissipation of liquid metal on the solid surface is achieved.

CN118910550APending Publication Date: 2024-11-08YUNNAN KEWEI LIQUID METAL VALLEY R & D CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410968333.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Liquid metal has poor wetting ability on most solid surfaces, resulting in a high interface thermal resistance between the solid surface and the liquid metal, affecting the heat dissipation efficiency.

Method used

The composite coating structure is adopted, including the arrangement of a highly thermally conductive intermediate layer and an infiltration layer on the solid surface. The intermediate layer and the liquid metal are intersoluble to form intermetallic compounds. The infiltration layer acts as a protective layer to avoid oxidation, improves the wettability of the liquid metal and reduces the interface heat. Obstacle.

Benefits of technology

It significantly improves the wettability of liquid metal to the solid surface, reduces the contact thermal resistance between the solid surface and the liquid metal, enhances thermal conductivity, and maintains stability during the aging process to prevent the coating from falling off.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910550A_ABST
    Figure CN118910550A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of heat dissipation of electronic devices, in particular to a composite coating and application of the composite coating to improvement of wettability of liquid metal to the surface of a solid matrix. The composite coating comprises a solid substrate, a middle layer arranged on the surface of the solid substrate and an infiltration layer arranged on the surface of the middle layer. According to the composite coating, the wettability of the liquid metal and the solid surface can be remarkably improved, large-area spreading of the liquid metal on the solid surface is achieved, the contact thermal resistance between the solid surface and the liquid metal interface is remarkably reduced, and the composite coating has excellent stability and good heat conduction performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of heat dissipation of electronic devices, and in particular to a composite coating and an application thereof in improving the wettability of liquid metal on the surface of a solid substrate. Background Art

[0002] As electronic devices continue to develop towards miniaturization and integration, their "thermal barrier" problem has become increasingly prominent. The heating problem has become one of the important challenges for electronic devices to develop higher performance. The development of new high-performance cooling technology is imminent. Liquid metal refers to a large class of multi-metal alloy functional materials with a melting point near room temperature. It has the characteristics of high thermal conductivity, strong electrical conductivity, good fluidity, wide liquid phase temperature range, easy to achieve flexible solid-liquid conversion, good stability, environmental protection and non-toxicity. Its inherent high thermal conductivity gives it excellent heat transfer performance, and its excellent stability expands the ultimate heat flux density that can be achieved by water cooling technology. It is a very potential thermal management solution. After years of development, liquid metal cooling technology has been continuously improved and extended to form its unique technical system. Convection cooling technology based on liquid metal, liquid metal thermal interface material technology and low melting point metal phase change temperature control technology have all achieved an order of magnitude improvement in cooling capacity compared to traditional cooling technology, bringing a new solution to the cooling of a large number of devices and equipment facing the problem of "thermal barrier". However, since liquid metal has a large surface tension (0.5-0.7N / m) and is easily oxidized, it has poor wetting ability on most solid surfaces and cannot spread on the solid surface. This can easily lead to high thermal resistance between the two interfaces, thereby affecting the heat transfer efficiency of the entire heat dissipation system.

[0003] The invention "Thermal interface and method for obtaining it, and method for promoting heat conduction" with application number CN202110401680.8 applies a single metal wetting layer that is miscible with liquid metal on the surface of the device, and prepares a rough surface on the surface of the metal wetting layer, and further improves the wettability between the wetting layer and the liquid metal through the capillary effect. Although the wetting material is miscible with the liquid metal and will spontaneously alloy to form intermetallic compounds, and the intermetallic compounds and liquid metal have natural good wettability due to the metal bond wetting mechanism, the generated intermetallic compounds have poor adhesion to the solid substrate, and will fall off over a large area during the aging process, leaking out of the solid surface that is not wetted by the liquid metal, resulting in a further increase in the interfacial thermal resistance. There are also studies that set a coating structure containing a metal Ti transition layer on the surface of a flexible film substrate. Although it can be used to solve the problem of difficulty in preparing conductive elements on the film surface, it is not suitable for heat dissipation and efficient heat conduction of electronic devices. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a composite coating and its application in improving the wettability of liquid metal on the surface of a solid substrate.

[0005] Specifically, the present invention adopts the following technical solutions: In a first aspect, the present invention provides a composite coating for improving the wettability of liquid metal to a solid surface, the composite coating comprising a solid substrate, an intermediate layer disposed on the surface of the solid substrate, and a wetting layer disposed on the surface of the intermediate layer. The composite coating provided by the present invention can significantly improve the wettability of liquid metal to the solid surface, achieve large-area spreading of liquid metal on the solid surface, significantly reduce the contact thermal resistance between the two interfaces of the solid surface and the liquid metal, and the composite coating has excellent stability and good thermal conductivity.

[0006] Preferably, the intermediate layer is a metal or alloy with high thermal conductivity and corrosion resistance to liquid metal. In the present invention, the intermediate layer is located between the solid (substrate) surface and the wetting layer, has high thermal conductivity, the wettability of the wetting layer to liquid metal is stronger than the wettability of the intermediate layer to liquid metal, and the intermediate layer can resist liquid metal corrosion within a certain temperature range.

[0007] The present invention improves the wettability of liquid metal on non-wetting solid surfaces by arranging a composite coating (wetting layer + intermediate layer) on the solid surface, and the composite coating has excellent stability and good thermal conductivity. After contacting with liquid metal, the wetting layer located on the top layer of the solid surface and the liquid metal will spontaneously alloy to generate intermetallic compounds. At the same time, the wetting layer also serves as a protective layer for the intermediate layer to avoid oxidation of the intermediate layer. When the wetting layer and the liquid metal are mutually dissolved and disappear, the generated intermetallic compounds and liquid metal can quickly wet the active intermediate layer, thereby achieving large-area spreading of liquid metal on the solid surface and significantly reducing the thermal resistance between the two interfaces of the solid surface and the liquid metal; the intermediate layer can resist liquid metal corrosion within a certain temperature range, so that the wetting performance of this composite coating is stable, and the coating will not fall off during the aging process.

[0008] Preferably, the intermediate layer includes one or more of Co, W, Ni, Mo, Mn, Si, and Pt.

[0009] Preferably, the thickness of the intermediate layer is 0.001 to 5 microns, preferably 0.1 to 4 microns.

[0010] Preferably, the wetting layer is miscible with the liquid metal, or the wetting layer is an intermetallic compound having wettability with the liquid metal. The wetting layer selected in the present invention is related to the type of liquid metal in contact, and the selected wetting layer material must have wettability with the liquid metal. In the present invention, the wetting layer is located on the top layer of the surface of the solid substrate, directly in contact with the liquid metal, the wetting layer has a certain degree of mutual solubility with the liquid metal, and can spontaneously react with the liquid metal to form an alloy, or the wetting layer is the product of the alloying reaction between the liquid metal and other metals - an intermetallic compound, which has good wettability with the liquid metal due to the metal bond wetting mechanism.

[0011] Further preferably, the wetting layer comprises an alloy of one or more of Cu, Ni, Ag, Au, Mg, Al, In, Zn, Fe, Sn, and Ga; or the wetting layer is an intermetallic compound of liquid metal, and the intermetallic compound of liquid metal is selected from one or more of intermetallic compounds of gallium-M, indium-M or tin-M; preferably, the M is selected from one or more of silver, copper, gold, zinc, aluminum, tungsten, nickel, iron, magnesium, manganese, platinum, titanium, bismuth or molybdenum, and more preferably, the M is silver and / or copper.

[0012] Preferably, the thickness of the wetting layer is 0.001-5 microns, preferably 0.5-4 microns.

[0013] Preferably, the melting point of the liquid metal is 3-250°C.

[0014] Further preferably, the liquid metal includes one or more of pure gallium, gallium-based liquid metal, indium-based liquid metal, and bismuth-based liquid metal.

[0015] Preferably, the solid matrix includes Si, a metal matrix or a ceramic matrix.

[0016] Further preferably, the metal matrix includes copper, aluminum or stainless steel.

[0017] Further preferably, the ceramic matrix includes Al2O3, ZrO2, Si3N4 or SiC.

[0018] Preferably, the wetting layer and the intermediate layer are prepared by a thin film deposition process; the thin film deposition process preferably includes one or more of plasma enhanced chemical vapor deposition, magnetron sputtering, electron beam evaporation and vacuum evaporation.

[0019] Preferably, the surface of the wetting layer is roughened. According to the Wenzel contact angle model, increasing the roughness will make the hydrophilic surface more hydrophilic, and the surface of the wetting layer can be roughened to improve its wettability with the liquid metal. The roughening treatment preferably includes one or more of solvent etching, electrochemical sandblasting and plasma etching. The present invention further improves the wettability of the wetting layer with the liquid metal by performing the above-mentioned roughening treatment on the surface of the wetting layer.

[0020] The second invention, the present invention also provides the application of the above-mentioned composite coating in improving the wettability of liquid metal to the surface of a solid substrate; preferably, when the liquid metal is used as an interface material heat transfer medium, a phase change temperature control material or a fluid heat dissipation medium, the composite coating is arranged on the surface of the device in direct contact with the liquid metal, which is used to increase the wettability between the liquid metal and the device surface, reduce the contact thermal resistance of the interface, improve the efficiency of heat conduction, and achieve rapid heat dissipation of the heat source; or when the liquid metal is used as a hydraulic transmission medium or a lubricant, the composite coating is used to reduce the friction between the liquid metal and the device surface and increase the lubricity between materials. The application includes when the liquid metal is used as an interface material heat transfer medium, a phase change temperature control material, or a fluid heat dissipation medium, the composite coating can be arranged on the surface of the device in direct contact with the liquid metal, which can increase the wettability between the liquid metal and the device surface, reduce the contact thermal resistance of the two interfaces, and improve the efficiency of heat conduction, thereby achieving rapid heat dissipation of the heat source; when the liquid metal is used as a hydraulic transmission medium or a lubricant, the composite coating can also reduce the friction between the liquid metal and the device surface and increase the lubricity between materials.

[0021] The beneficial effect of the present invention is at least that: the present invention improves the wettability of liquid metal on non-wetting solid surfaces by setting a composite coating (wetting layer + intermediate layer) on the solid surface. After contacting with liquid metal, the wetting layer located on the top layer of the solid surface will spontaneously alloy with the liquid metal to generate intermetallic compounds. At the same time, the wetting layer also serves as a protective layer for the intermediate layer to avoid oxidation of the intermediate layer. When the wetting layer and the liquid metal are mutually dissolved and disappear, the generated intermetallic compounds and liquid metal can quickly wet the active intermediate layer, thereby achieving large-area spreading of liquid metal on the solid surface. The intermediate layer can resist liquid metal corrosion within a certain temperature range, resulting in stable wetting performance of the composite coating, and no coating shedding will occur during the aging process. The process of the present invention is simple, the composite coating has universal applicability to solid surfaces, and at the same time has good thermal conductivity and wetting properties, and has strong industrial promotion and implementation. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0023] Figure 1 A schematic structural diagram of a composite coating provided in an embodiment of the present invention.

[0024] Figure 2 In Example 6 of the present invention, in liquid metal Ga 86.5 Sn 13.5 In the wetting test, the SiC sample is vertically immersed in the liquid metal for 3 seconds and then picked up, and the liquid metal spreads over a large area on the surface of the specimen.

[0025] Figure 3 This is the elemental analysis of the coating surface of Example 6 of the present invention after 144 hours of high and low temperature aging test.

[0026] Figure 4 This is the elemental analysis of the coating surface of Comparative Example 7 of the present invention after 144 hours of high and low temperature aging test.

[0027] Among them, 1-solid substrate; 2-intermediate layer; 3-wetting layer. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the drawings of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Example 1

[0030] This embodiment provides a (Ni+Cu) composite coating, such as Figure 1 As shown, the composite coating includes a solid substrate 1, an intermediate layer 2 and a wetting layer 3. High-purity Ni and Cu target materials are selected, and the intermediate layer Ni layer and the wetting layer Cu layer are successively deposited on the surface of the Al material of the heat dissipation device with a roughness of 0.01μm by magnetron sputtering process. The deposition thickness of the intermediate layer Ni layer is 3 microns, and the deposition thickness of the wetting layer Cu layer is 3 microns.

[0031] Then, the composite coating was roughened by Ar plasma for 5 min.

[0032] Example 2

[0033] The present embodiment provides a (Co+Ag) composite coating, which uses high-purity Co and Ag target materials, and uses a magnetron sputtering process to successively deposit an intermediate layer Co layer and a wetting layer Ag layer on the surface of a Cu material of a heat dissipation device with a roughness of 0.01 μm. The deposition thickness of the intermediate layer Co layer is 3 microns, and the deposition thickness of the wetting layer Ag layer is 3 microns.

[0034] Then, the composite coating was roughened by Ar plasma for 5 min.

[0035] Example 3

[0036] This embodiment provides a (W+CuGa2) composite coating, which uses high-purity W and CuGa2 target materials (the molar ratio of Cu to Ga is 1:2), and uses a magnetron sputtering process to successively deposit an intermediate layer W layer and an infiltration layer CuGa2 layer on the surface of a ceramic Si3N4 substrate with a roughness of 0.01μm. The deposition thickness of the intermediate layer W layer is 3 microns, and the deposition thickness of the infiltration layer CuGa2 layer is 3 microns.

[0037] Then, the composite coating was roughened by Ar plasma for 5 min.

[0038] Example 4

[0039] This embodiment provides a (Ni+Cu) composite coating, which uses high-purity Ni and Cu target materials, and uses a magnetron sputtering process to successively deposit an intermediate Ni layer and a wetting Cu layer on the surface of a ceramic substrate SiC with a roughness of 0.01 μm. The deposition thickness of the intermediate Ni layer is 1 micron, and the deposition thickness of the wetting Cu layer is 2 microns.

[0040] Then, the composite coating was roughened by Ar plasma for 10 min.

[0041] Example 5

[0042] The present embodiment provides a (Si+CuGa2) composite coating, which uses high-purity Si and CuGa2 target materials (the molar ratio of Cu to Ga is 1:2), and uses a magnetron sputtering process to successively deposit an intermediate Si layer and a wetting CuGa2 layer on the surface of a ceramic substrate SiC with a roughness of 0.01μm. The deposition thickness of the intermediate Si layer is 0.5 microns, and the deposition thickness of the wetting CuGa2 layer is 2 microns.

[0043] Then, the composite coating was roughened by Ar plasma for 10 min.

[0044] Example 6

[0045] This embodiment provides a (Mo+Cu) composite coating, which uses high-purity Mo and Cu target materials, and uses a magnetron sputtering process to successively deposit an intermediate Mo layer and a wetting Cu layer on the surface of a ceramic substrate SiC with a roughness of 0.01 μm. The deposition thickness of the intermediate Mo layer is 1 micron, and the deposition thickness of the wetting Cu layer is 2 microns.

[0046] Then, the composite coating was roughened by Ar plasma for 10 min.

[0047] Comparative Example 1

[0048] Compared with Example 1, Comparative Example 1 did not use Ar plasma to roughen the surface of the composite coating.

[0049] Comparative Example 2

[0050] Compared with Example 2, in Comparative Example 1, no wetting layer was formed, and only the middle layer Co layer was deposited.

[0051] Comparative Example 3

[0052] Compared with Example 3, Comparative Example 2 did not have a wetting layer, and only deposited an intermediate layer W.

[0053] Comparative Example 4

[0054] Uncoated Si3N4 ceramic substrate.

[0055] Comparative Example 5

[0056] Compared with Example 4, the intermediate layer of Comparative Example 6 is a Ti layer.

[0057] Comparative Example 6

[0058] Uncoated SiC ceramic substrate.

[0059] Comparative Example 7

[0060] Compared with Example 6, in Comparative Example 7, no intermediate layer was formed, and only the wetting layer Cu layer was deposited.

[0061] Performance Evaluation

[0062] (1) Wettability test: Contact angle tests were performed on Examples 1-3 and Comparative Examples 1-4. The test standard was Q / LMJC101-2022. The image of a drop of liquid metal falling on the surface of the substrate was captured and the contact angle was measured. The liquid metal was gallium indium tin with a mass ratio of Ga 62.5 In 21.5 Sn 16 , melting point is 11°C, and the test data are shown in Table 1.

[0063]

[0064] It can be seen from the data in Table 1 that the wetting layer in the composite coating provided by the embodiment of the present invention can significantly reduce the contact angle between the liquid metal and the solid surface, realize the large-area spreading of the liquid metal on the solid surface, and make the non-wetting solid surface and the liquid metal present good wettability. It can be seen from the contact angles of Example 1 and Comparative Example 1 that roughening the composite coating can reduce the contact angle between the liquid metal and the composite coating, and further improve the wettability of the liquid metal and the solid surface. Figure 2 In Example 6, the mass ratio of Ga 86.5 Sn 13.5 In the wetting test, the SiC sample was vertically immersed in the liquid metal for 3 seconds and then picked up. The liquid metal evenly covered the entire surface of the sample coated with the composite coating, and a large area of ​​liquid metal was spread on the surface of the specimen. And this composite coating structure of intermediate layer + infiltration layer is universal and applicable to both metal substrates and ceramic substrates. Only the contact angle between the single metal coating in the intermediate layer and the liquid metal did not decrease significantly, because the metal in the intermediate layer was oxidized, and the generated oxide film did not wet the liquid metal, resulting in a relatively large contact angle.

[0065] (2) Interface thermal resistance test: Thermal resistance tests were performed on Examples 4-6 and Comparative Examples 5-6. The test standard was ASTM D5470-17, the pressure was 30 psi, the test sample temperature was 60°C, the non-steady-state rate was less than 5%, the liquid metal was gallium tin, and the mass ratio was Ga 86.5 Sn 13.5 , the melting point is 20.5℃, and the test data are shown in Table 2.

[0066]

[0067] It can be seen from the data in Table 2 that, compared with the SiC ceramic substrate without any coating treatment, the composite coating provided by the embodiment of the present invention has good wettability with the liquid metal, and the intermediate layer has a high thermal conductivity and good thermal conductivity. There is a small interface thermal resistance between the liquid metal and the coating, so it can significantly improve the efficiency of heat conduction, thereby realizing rapid heat dissipation of the heat source. However, the thermal conductivity of the intermediate layer Ti of Comparative Example 5 is not high, resulting in a high interface thermal resistance, which is not conducive to efficient heat conduction.

[0068] (3) Reliability test: Example 6 and Comparative Example 7 were encapsulated in liquid metal gallium tin with a mass ratio of Ga 86.5 Sn 13.5, and then carry out high and low temperature thermal shock accelerated aging test, the temperature range is -40℃~120℃, the high temperature and low temperature insulation time are 30min respectively, the switching time is about 5s, and the number of aging cycles is 144 times (1h / time). After the aging test is completed, the sample is cleaned with alcohol, and finally the coating surface is analyzed by SEM scanning electron microscope. The relevant information of test example 6 and comparative example 7 is shown in Table 3, and the surface element analysis after aging is shown in Figure 3 and Figure 4 .

[0069]

[0070] from Figure 3 , Figure 4 The elements on the coating surface show that the wetting layer Cu in the composite coating of Example 6 "disappears" after alloying with the liquid metal, but E-(GaSn) firmly covers the middle layer Mo and covers the entire sample surface; while in Comparative Example 7, after the wetting layer Cu reacts with the liquid metal, E-(GaSn) is only partially attached to the sample surface, and most of the SiC matrix that is not wetted by the liquid metal is leaked. The wetting performance of the composite coating structure provided by the embodiment of the present invention is more stable and reliable.

[0071] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A composite coating, characterized in that: The invention comprises a solid substrate, an intermediate layer arranged on the surface of the solid substrate and an infiltration layer arranged on the surface of the intermediate layer.

2. The composite coating according to claim 1, characterized in that: The intermediate layer is a metal or alloy having high thermal conductivity and corrosion resistance to liquid metal; preferably, the intermediate layer includes one or more of Co, W, Ni, Mo, Mn, Si, and Pt.

3. The composite coating according to claim 2, characterized in that: The thickness of the intermediate layer is 0.001-5 microns.

4. The composite coating according to any one of claims 1 to 3, characterized in that: The wetting layer is mutually soluble in the liquid metal, or the wetting layer is an intermetallic compound having wettability with the liquid metal.

5. The composite coating according to claim 4, characterized in that: The wetting layer includes an alloy of one or more of Cu, Ni, Ag, Au, Mg, Al, In, Zn, Fe, Sn, and Ga; or the wetting layer is an intermetallic compound of liquid metal, and the intermetallic compound of liquid metal is selected from one or more intermetallic compounds of gallium-M, indium-M or tin-M; preferably, the M is selected from one or more of silver, copper, gold, zinc, aluminum, tungsten, nickel, iron, magnesium, manganese, platinum, titanium, bismuth or molybdenum, and more preferably, the M is silver and / or copper.

6. The composite coating according to claim 4 or 5, characterized in that: The thickness of the wetting layer is 0.001-5 microns.

7. The composite coating according to any one of claims 1 to 6, characterized in that: The melting point of the liquid metal is 3-250° C.; the liquid metal includes one or more of pure gallium, gallium-based liquid metal, indium-based liquid metal, and bismuth-based liquid metal.

8. The composite coating according to any one of claims 1 to 7, characterized in that: The solid matrix includes Si, a metal matrix or a ceramic matrix; Preferably, the metal matrix includes copper, aluminum or stainless steel; the ceramic matrix includes Al2O3, ZrO2, Si3N4 or SiC.

9. The composite coating according to any one of claims 1 to 8, characterized in that: The wetting layer and the intermediate layer are prepared by a thin film deposition process; the thin film deposition process preferably includes one or more of plasma enhanced chemical vapor deposition, magnetron sputtering, electron beam evaporation and vacuum evaporation; Preferably, the surface of the wetting layer is roughened; the roughening treatment preferably includes one or more of solvent etching, electrochemical sandblasting and plasma etching.

10. An application of the composite coating according to any one of claims 1 to 9 in improving the wettability of liquid metal on the surface of a solid substrate; preferably, when the liquid metal is used as an interface material heat transfer medium, a phase change temperature control material or a fluid heat dissipation medium, the composite coating is arranged on the surface of the device in direct contact with the liquid metal, so as to increase the wettability between the liquid metal and the device surface, reduce the contact thermal resistance of the interface, improve the efficiency of heat conduction, and realize rapid heat dissipation of the heat source; or when the liquid metal is used as a hydraulic transmission medium or a lubricant, the composite coating is used to reduce the friction between the liquid metal and the device surface and increase the lubricity between the materials.

Citation Information

Cited By

  • Negative-wear super-wear-resistant current-carrying friction pair material