High-flexibility polylactic acid fabric and production process thereof

High-flexibility polylactic acid (PLA) fabrics were prepared by cross-linking blending and blending technology, which solved the brittleness problem of PLA fibers, enhanced their toughness and antibacterial properties, and achieved efficient antibacterial and heat-resistant effects.

CN118910792APending Publication Date: 2024-11-08JIE SHOU SHI SAN BAO XIAN YE YOU XIAN ZE REN GONG SI
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410996721.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Polylactic acid fiber suffers from high brittleness and low toughness, which limits its application in certain fields, and the antibacterial properties of existing antibacterial agents are not long-lasting.

Method used

Polylactic acid (PLA) is mixed with polycaprolactone (PVC) and thermotropic liquid crystal polymers via cross-linking blending to form a network structure. Chitosan fiber and hemp fiber are then added for blending to prepare a highly flexible PLA fabric, utilizing the antibacterial properties of chitosan and the antibacterial, moisture-wicking, and breathable properties of hemp fiber.

Benefits of technology

It improves the toughness and heat resistance of polylactic acid fibers, enhances the antibacterial and deodorizing properties of the fabric, improves the softness and ease of cleaning of the fabric, and has excellent antibacterial effect and heat resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004960438000000091
    Figure BDA0004960438000000091
Patent Text Reader

Abstract

The invention discloses a high-flexibility polylactic acid fabric and a production process thereof, and belongs to the technical field of textile, modified polylactic acid fibers are prepared by a crosslinking blending method, and the modified polylactic acid fibers, chitosan fibers and hemp fibers are blended to prepare the high-flexibility polylactic acid fabric. Polylactic acid and polycaprolactone are crosslinked under the action of a cross-linking agent to form polylactic acid of a net structure, the polylactic acid is further blended with the thermotropic liquid crystal polymer at high temperature, a microfiber structure is formed in situ to prevent crack expansion, the toughness of the fabric is improved through the combined action, and the thermotropic liquid crystal polymer is good in heat resistance and can avoid negative effects on the heat resistance of polylactic acid. The chitosan fiber and the China hemp fiber are added, and different antibacterial mechanisms of the chitosan fiber and the China hemp fiber are comprehensively utilized, so that efficient antibacterial performance is achieved, high-flexibility polylactic acid fabric with different patterns can be further formed by a jacquard knitting machine, and the fabric can be widely applied to the fields of home textiles and clothes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of textiles, and in particular relates to a high-flexibility polylactic acid fabric and a production process thereof. Background Art

[0002] Polylactic acid (PLA) is a new type of bio-based and renewable biodegradable material, made from starch raw materials extracted from renewable plant resources (such as corn, cassava, etc.). Polylactic acid fiber is made of polylactic acid through polycondensation and melt spinning. Polylactic acid fiber has good biodegradability, moisture absorption and moisture conductivity, antibacterial and flame retardancy. Clothing made of polylactic acid fiber has good environmental adaptability and can alleviate the environmental pollution caused by the production process of textiles and clothing to a large extent.

[0003] Although polylactic acid fiber has good mechanical properties, its low elongation at break (usually less than 10%) and poor toughness limit its widespread use in certain specific fields. For the preparation of fabrics, the high brittleness of PLA becomes its fatal disadvantage. From the structure of PLA, it can be seen that the carbonyl group in the PLA molecular chain is coplanar with the adjacent oxygen atom and is very close to the adjacent carbon atom, making it difficult to rotate. The molecular chain has poor flexibility, and the material is hard and brittle, with poor impact resistance.

[0004] In order to solve the shortcomings of high brittleness and low toughness of polylactic acid, the main methods tried in current research include various technologies such as chemical copolymerization, plasticization and blending for toughening. Poly(ε-caprolactone) (PCL) is a water-insoluble, biodegradable aliphatic polyester, which is often blended with PLLA to improve its brittleness. At present, some research and exploration have been carried out on the use of polycaprolactone to toughen polylactic acid. Toughening polylactic acid without affecting sustainability has good development prospects, but there are also defects. From the perspective of processing and heat resistance, polylactic acid still has defects such as slow crystallization rate and low heat deformation temperature after toughening treatment, which will limit the wide application of polylactic acid. Therefore, it is necessary to start with the selection of materials and preparation process to study the toughening of polylactic acid, and also consider the crystallization rate and heat deformation temperature.

[0005] During the use of polylactic acid fabrics in the fields of home textiles and clothing, they are easily contaminated by human sweat and produce bacteria, posing a threat to human health. Therefore, the development of polylactic acid fiber antibacterial fabrics is very necessary. The polylactic acid antibacterial textiles prepared by adding antibacterial agents have certain antibacterial properties, but after long-term use, their antibacterial properties will gradually decrease, and the antibacterial long-term effect is low. Summary of the invention

[0006] The object of the present invention is to provide a high-flexibility polylactic acid fabric and a production process thereof, so as to solve the problem of low toughness of the polylactic acid fabric.

[0007] The purpose of the present invention can be achieved through the following technical solutions:

[0008] The invention provides a high-flexibility polylactic acid fabric, which is knitted by jacquard knitting warp yarns and weft yarns;

[0009] The warp yarn raw material includes 32-40 parts by weight of modified polylactic acid fiber and 4-10 parts of hemp fiber;

[0010] The weft yarn raw material includes 32-40 parts by weight of modified polylactic acid fiber and 4-10 parts by weight of chitosan fiber;

[0011] The modified polylactic acid fiber is prepared by melt spinning after cross-linking and blending 60-80 parts of polylactic acid, 10-20 parts of polycaprolactone, 0.5-3 parts of a cross-linking agent and 5-15 parts of a thermotropic liquid crystal polymer by weight.

[0012] Furthermore, the cross-linking agent is any one of dicumyl peroxide, benzoyl peroxide and 3-isocyanatepropyltriethoxysilane.

[0013] Furthermore, the thermotropic liquid crystal polymer is type III LCP, which has a lower thermal deformation temperature than type I and type II, and has a lower melting temperature requirement, so it is easy to melt blend with polylactic acid.

[0014] The present invention also provides a production process of a high-flexibility polylactic acid fabric as described in any one of claims 1 to 5, comprising the following steps:

[0015] (1) Spinning: 60-80 parts of polylactic acid, 10-20 parts of polycaprolactone and 0.5-3 parts of a crosslinking agent are mixed at 160-170°C and subjected to a crosslinking reaction for 3-4 hours. The mixture is heated to 210-240°C and 5-15 parts of a thermotropic liquid crystal polymer are added and melt-spun to prepare modified polylactic acid fibers. The thermotropic liquid crystal polymer has a high melting point and needs to be heated to melt and form a fluid state before being blended with polylactic acid. Full contact is conducive to the in-situ formation of a microfiber structure.

[0016] (2) Blended yarn: The warp yarn is prepared by blending 32-40 parts of modified polylactic acid fiber and 4-10 parts of hemp fiber, and the weft yarn is prepared by blending 32-40 parts of modified polylactic acid fiber and 4-10 parts of chitosan fiber, and dyeing treatment is performed to prepare yarns of different colors. After adding chitosan and hemp fiber, polar hydrophilic groups exist on the surface of the fabric, which can improve the dyeing effect and facilitate cleaning;

[0017] (3) Weaving: Warp and weft yarns are knitted by jacquard knitting machines to prepare fabrics;

[0018] (4) Post-processing: The fabric is washed, shaped, singed and then rolled up.

[0019] Furthermore, the jacquard knitting machine is a double-sided jacquard circular machine.

[0020] Furthermore, the water washing temperature is 60-80°C.

[0021] Furthermore, the shaping temperature is 110-120° C., and the shaping speed is 8-10 m / min.

[0022] Furthermore, the singeing temperature is 140° C. Too high a singeing temperature will cause the fabric to turn yellow.

[0023] Beneficial effects of the present invention:

[0024] (1) Through the cross-linking blending method, polylactic acid and polycaprolactone are cross-linked under the action of a cross-linking agent to form polylactic acid with a network structure, which can improve toughness and promote polylactic acid crystallization. Adding thermotropic liquid crystal polymer for blending, the thermotropic liquid crystal polymer will form a microfiber structure in situ during the melt processing process, which can prevent crack propagation and further improve the toughness of polylactic acid fibers. Thermotropic liquid crystal polymer has a high thermal deformation temperature, which is conducive to ensuring the heat resistance of polylactic acid.

[0025] (2) Chitosan fiber is added to polylactic acid fiber for blending. Chitosan contains polar groups such as hydroxyl and amino groups, which can enhance the hydrophilicity of the fabric and facilitate fabric dyeing and cleaning. It carries a positive charge and binds to bacterial protein to modify it and cause the bacteria to flocculate and precipitate, thereby inhibiting its reproduction ability. It has a significant antibacterial effect mainly on Gram-positive bacteria, giving the fabric antibacterial and deodorizing properties.

[0026] (3) Hemp fiber has good heat resistance and toughness. Its cross-section is an irregular polygon, triangle, etc. The central cavity is linear or elliptical, which can block ultraviolet radiation. It contains phenolic substances that can effectively kill mold microorganisms. The top of the hemp fiber is blunt and round, and has a soft feel. The blended fabric is antibacterial, moisture-absorbent and breathable. DETAILED DESCRIPTION

[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] Example 1

[0029] Spinning: 80 parts of polylactic acid, 10 parts of polycaprolactone and 2 parts of benzoyl peroxide were weighed by mass and added to the reactor, stirred and mixed at a constant temperature of 170°C, and the cross-linking reaction was continued for 4 hours. Then, the mixture was put into a screw extruder, and 5 parts of Rodrun LC-3000 were added and stirred and blended. The temperature was raised to 220°C for melt extrusion spinning, and the drafting ratio was 3.3 to obtain modified polylactic acid fiber.

[0030] Blended yarn: 40 parts of modified polylactic acid fiber and 10 parts of hemp fiber were weighed by weight to prepare warp yarn, and 40 parts of modified polylactic acid fiber and 10 parts of chitosan fiber were blended to prepare weft yarn, and then dyed to prepare brown and white yarns;

[0031] Weaving: Warp and weft yarns are used to prepare fabrics by double-sided jacquard circular knitting machines;

[0032] Post-treatment: the fabric is washed at 80°C, and after washing for 30 minutes, it is shaped at 120°C, and the shaping speed is set to 8m / min. The shaped fabric is singed, and the singeing roller is set to 140°C. The fabric is wound up by the winding roller to obtain the fabric.

[0033] Example 2

[0034] Spinning: Weigh 80 parts of polylactic acid, 10 parts of polycaprolactone and 2 parts of benzoyl peroxide by mass and add them to the reactor, stir and mix at a constant temperature of 170°C, continue the cross-linking reaction for 4 hours, then put them into the screw extruder, add 10 parts of Rodrun LC-3000 and stir and blend, heat to 220°C for melt extrusion spinning, and the drafting ratio is 3.3 to obtain modified polylactic acid fiber.

[0035] Blended yarn: 40 parts of modified polylactic acid fiber and 10 parts of hemp fiber were weighed by weight to prepare warp yarn, and 40 parts of modified polylactic acid fiber and 10 parts of chitosan fiber were blended to prepare weft yarn, and then dyed to prepare brown and white yarns;

[0036] Weaving: Warp and weft yarns are used to prepare fabrics by double-sided jacquard circular knitting machines;

[0037] Post-treatment: the fabric is washed at 80°C, and after washing for 30 minutes, it is shaped at 120°C, and the shaping speed is set to 8m / min. The shaped fabric is singed, and the singeing roller is set to 140°C. The fabric is wound up by the winding roller to obtain the fabric.

[0038] Example 3

[0039] Spinning: Weigh 80 parts of polylactic acid, 10 parts of polycaprolactone and 2 parts of benzoyl peroxide by mass and add them to the reactor, stir and mix at a constant temperature of 170°C, continue the cross-linking reaction for 4 hours, then put them into the screw extruder, add 15 parts of Rodrun LC-3000 and stir and blend, heat to 220°C for melt extrusion spinning, and the drafting ratio is 3.3 to obtain modified polylactic acid fiber.

[0040] Blended yarn: 40 parts of modified polylactic acid fiber and 10 parts of hemp fiber were weighed by weight to prepare warp yarn, and 40 parts of modified polylactic acid fiber and 10 parts of chitosan fiber were blended to prepare weft yarn, and then dyed to prepare brown and white yarns;

[0041] Weaving: Warp and weft yarns are used to prepare fabrics by double-sided jacquard circular knitting machines;

[0042] Post-treatment: the fabric is washed at 80°C, and after washing for 30 minutes, it is shaped at 120°C, and the shaping speed is set to 8m / min. The shaped fabric is singed, and the singeing roller is set to 140°C. The fabric is wound up by the winding roller to obtain the fabric.

[0043] Example 4

[0044] Spinning: 80 parts of polylactic acid, 10 parts of polycaprolactone and 2 parts of benzoyl peroxide were weighed by mass and added to a reactor. The mixture was stirred and mixed at a constant temperature of 170°C. After the cross-linking reaction was continued for 4 hours, the mixture was put into a screw extruder, and 20 parts of Rodrun LC-3000 were added and stirred and blended. The temperature was raised to 220°C for melt extrusion spinning. The draft ratio was 3.3 to obtain modified polylactic acid fiber.

[0045] Blended yarn: 40 parts of modified polylactic acid fiber and 10 parts of hemp fiber were weighed by weight to prepare warp yarn, and 40 parts of modified polylactic acid fiber and 10 parts of chitosan fiber were blended to prepare weft yarn, and then dyed to prepare brown and white yarns;

[0046] Weaving: Warp and weft yarns are used to prepare fabrics by double-sided jacquard circular knitting machines;

[0047] Post-treatment: the fabric is washed at 80°C, and after washing for 30 minutes, it is shaped at 120°C, and the shaping speed is set to 8m / min. The shaped fabric is singed, and the singeing roller is set to 140°C. The fabric is wound up by the winding roller to obtain the fabric.

[0048] Example 5

[0049] Spinning: 80 parts of polylactic acid, 10 parts of polycaprolactone and 2 parts of benzoyl peroxide were weighed and added to the reactor, stirred and mixed at a constant temperature of 170°C, and the cross-linking reaction was continued for 4 hours before being put into the screw extruder. 15 parts of A430 was stirred and blended, heated to 220°C for melt extrusion spinning, and the draft ratio was 3.3 to obtain modified polylactic acid fiber.

[0050] Blended yarn: 40 parts of modified polylactic acid fiber and 10 parts of hemp fiber were weighed by weight to prepare warp yarn, and 40 parts of modified polylactic acid fiber and 10 parts of chitosan fiber were blended to prepare weft yarn, and then dyed to prepare brown and white yarns;

[0051] Weaving: Warp and weft yarns are used to prepare fabrics by double-sided jacquard circular knitting machines;

[0052] Post-treatment: the fabric is washed at 80°C, and after washing for 30 minutes, it is shaped at 120°C, and the shaping speed is set to 8m / min. The shaped fabric is singed, and the singeing roller is set to 140°C. The fabric is wound up by the winding roller to obtain the fabric.

[0053] Comparative Example 1

[0054] The modified polylactic acid raw material is different from that in Example 1, and no polycaprolactone and cross-linking agent are added.

[0055] Spinning: 80 parts of polylactic acid were weighed by mass and put into a screw extruder, 5 parts of Rodrun LC-3000 were added and stirred and blended, and the temperature was raised to 220°C for melt extrusion spinning with a draft ratio of 3.3 to obtain modified polylactic acid fibers.

[0056] Blended yarn: 40 parts of modified polylactic acid fiber and 10 parts of hemp fiber were weighed by weight to prepare warp yarn, and 40 parts of modified polylactic acid fiber and 10 parts of chitosan fiber were blended to prepare weft yarn, and then dyed to prepare brown and white yarns;

[0057] Weaving: Warp and weft yarns are used to prepare fabrics by double-sided jacquard circular knitting machines;

[0058] Post-treatment: The fabric is washed at 80°C, and after washing for 30 minutes, it is shaped at 120°C. The shaping speed is set to 8m / min. The shaped fabric is singed, and the singeing roller is set to 140°C. After winding with a winding roller, a highly flexible polylactic acid fabric is obtained.

[0059] Comparative Example 2

[0060] The fiber raw material is different from that in Example 1, and the modified polylactic acid fiber is replaced by conventional polylactic acid fiber.

[0061] Blended yarn: 40 parts of polylactic acid fiber and 10 parts of hemp fiber were weighed by weight to prepare warp yarn, and 40 parts of polylactic acid fiber and 10 parts of chitosan fiber were blended to prepare weft yarn, and then dyed to prepare brown and white yarns;

[0062] Weaving: Warp and weft yarns are used to prepare fabrics by double-sided jacquard circular knitting machines;

[0063] Post-treatment: the fabric is washed at 80°C, and after washing for 30 minutes, it is shaped at 120°C, and the shaping speed is set to 8m / min. The shaped fabric is singed, and the singeing roller is set to 140°C. The fabric is wound up by the winding roller to obtain the fabric.

[0064] Comparative Example 3

[0065] The fiber raw material is different from that in Example 1, and the hemp fiber in the warp yarn is replaced by chitosan fiber.

[0066] Spinning: 80 parts of polylactic acid, 10 parts of polycaprolactone and 2 parts of benzoyl peroxide were weighed by mass and added to the reactor, stirred and mixed at a constant temperature of 170°C, and the cross-linking reaction was continued for 4 hours. Then, the mixture was put into a screw extruder, and 5 parts of Rodrun LC-3000 were added and stirred and blended. The temperature was raised to 220°C for melt extrusion spinning, and the drafting ratio was 3.3 to obtain modified polylactic acid fiber.

[0067] Blended yarn: 40 parts of modified polylactic acid fiber and 10 parts of chitosan fiber were weighed by weight to prepare warp yarn, and 40 parts of modified polylactic acid fiber and 10 parts of chitosan fiber were blended to prepare weft yarn, and then dyed to prepare brown and white yarns;

[0068] Weaving: Warp and weft yarns are used to prepare fabrics by double-sided jacquard circular knitting machines;

[0069] Post-treatment: the fabric is washed at 80°C, and after washing for 30 minutes, it is shaped at 120°C, and the shaping speed is set to 8m / min. The shaped fabric is singed, and the singeing roller is set to 140°C. The fabric is wound up by the winding roller to obtain the fabric.

[0070] Comparative Example 4

[0071] The fiber raw material is different from that in Example 1, the chitosan fiber in the weft yarn is replaced by hemp fiber, and the other steps are the same as in Example 1.

[0072] Spinning: 80 parts of polylactic acid, 10 parts of polycaprolactone and 2 parts of benzoyl peroxide were weighed by mass and added to the reactor, stirred and mixed at a constant temperature of 170°C, and the cross-linking reaction was continued for 4 hours. Then, the mixture was put into a screw extruder, and 5 parts of Rodrun LC-3000 were added and stirred and blended. The temperature was raised to 220°C for melt extrusion spinning, and the drafting ratio was 3.3 to obtain modified polylactic acid fiber.

[0073] Blended yarn: 40 parts of modified polylactic acid fiber and 10 parts of hemp fiber are weighed by weight to prepare warp yarn, and 40 parts of modified polylactic acid fiber and 10 parts of hemp fiber are blended to prepare weft yarn, and then dyed to prepare brown and white yarns;

[0074] Weaving: Warp and weft yarns are used to prepare fabrics by double-sided jacquard circular knitting machines;

[0075] Post-treatment: the fabric is washed at 80°C, and after washing for 30 minutes, it is shaped at 120°C, and the shaping speed is set to 8m / min. The shaped fabric is singed, and the singeing roller is set to 140°C. The fabric is wound up by the winding roller to obtain the fabric.

[0076] Comparative Example 5

[0077] The fiber raw material is different from that in Example 1, and pure polylactic acid fiber is used to prepare the fabric.

[0078] Blended yarn: pure polylactic acid fiber is used to prepare warp and weft yarns, and then dyed to prepare brown and white yarns;

[0079] Weaving: Warp and weft yarns are used to prepare fabrics by double-sided jacquard circular knitting machines;

[0080] Post-treatment: the fabric is washed at 80°C, and after washing for 30 minutes, it is shaped at 120°C, and the shaping speed is set to 8m / min. The shaped fabric is singed, and the singeing roller is set to 140°C. The fabric is wound up by the winding roller to obtain the fabric.

[0081] Performance tests were performed on Examples 1 to 5 and Comparative Examples 1 to 5, and the results are shown in Table 1.

[0082] The antibacterial performance test of fabrics refers to the standard test of GB / T 20994.3-2008 "Evaluation of Antibacterial Performance of Textiles";

[0083] The elongation at break test refers to GB / T 3923.1-2013 "Tensile properties of textile fabrics - Part 1: Determination of breaking strength and elongation at break (strip method)".

[0084] The tear strength test refers to GB / T 3917.1-2009 "Tear properties of textile fabrics - Part 1: Determination of tear strength by impact pendulum method".

[0085] Heat resistance test refers to GB / T 13767-1992 "Method for determination of heat resistance of textiles".

[0086] Table 1

[0087]

[0088] It can be seen from Table 1 that in Examples 1-3, as the content of Rodrun LC-3000 increases, the toughness of the modified polylactic acid fiber increases first and then decreases. When the added mass fraction is 15 parts, the toughness is the best, and the maximum tolerance temperature is increased to 140°C. The fabric prepared by A430 has good properties and excellent flexibility. Compared with Example 1, the polylactic acid in Comparative Example 1 did not undergo cross-linking reaction, and its toughness was significantly reduced. In Comparative Example 2, the conventional polylactic acid fiber was used to prepare the blended fabric. All properties except the antibacterial performance were reduced. In Comparative Examples 3 and 4, the fiber components in the warp and weft yarns were replaced respectively. When the warp and weft yarns were all chitosan fibers, the antibacterial performance of Aspergillus niger was poor. When the warp and weft yarns were all hemp fibers, the inhibition rate of Candida albicans decreased slightly, and the toughness of hemp fibers was better than that of chitosan fibers. The use of hemp fibers in the warp yarns was beneficial to the tear resistance of the fabric. In Comparative Example 5, the overall performance of the fabric prepared by using pure polylactic acid was significantly different from that of Examples 1-3. The fabric prepared in Example 3 had excellent comprehensive performance, high flexibility and high antibacterial properties, and good heat resistance.

[0089] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0090] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A highly flexible polylactic acid fabric, characterized in that: The high-flexibility polylactic acid fabric is formed by jacquard knitting of warp yarns and weft yarns; The warp yarn raw material includes 32-40 parts by weight of modified polylactic acid fiber and 4-10 parts of hemp fiber; The weft yarn raw material includes 32-40 parts by weight of modified polylactic acid fiber and 4-10 parts by weight of chitosan fiber; The modified polylactic acid fiber is prepared by melt spinning after cross-linking and blending 60-80 parts of polylactic acid, 10-20 parts of polycaprolactone, 0.5-3 parts of a cross-linking agent and 5-15 parts of a thermotropic liquid crystal polymer by weight.

2. The high-flexibility polylactic acid fabric according to claim 1, characterized in that: The crosslinking agent is any one of dicumyl peroxide, benzoyl peroxide and 3-isocyanate propyl triethoxy silane.

3. The high-flexibility polylactic acid fabric according to claim 1, characterized in that: The thermotropic liquid crystal polymer is type III LCP.

4. A production process for a high-flexibility polylactic acid fabric as claimed in any one of claims 1 to 3, characterized in that: The steps include: (1) Spinning: 60-80 parts of polylactic acid, 10-20 parts of polycaprolactone and 0.5-3 parts of a crosslinking agent are mixed at 160-170°C and subjected to a crosslinking reaction for 3-4 hours. The mixture is heated to 210-240°C and 5-15 parts of a thermotropic liquid crystal polymer are added and melt-spun to prepare modified polylactic acid fibers. (2) Blended yarn: The warp yarn is prepared by blending 32-40 parts of modified polylactic acid fiber and 4-10 parts of hemp fiber, and the weft yarn is prepared by blending 32-40 parts of modified polylactic acid fiber and 4-10 parts of chitosan fiber, and dyeing is performed to prepare yarns of different colors; (3) Weaving: Warp and weft yarns are knitted by jacquard knitting machines to prepare fabrics; (4) Post-processing: The fabric is washed, shaped, singed and then rolled up.

5. The production process of a high-flexibility polylactic acid fabric according to claim 4, characterized in that: The jacquard knitting machine is a double-sided jacquard circular machine.

6. The production process of a high-flexibility polylactic acid fabric according to claim 4, characterized in that: The water washing temperature is 60-80°C.

7. The production process of a high-flexibility polylactic acid fabric according to claim 4, characterized in that: The setting temperature is 110-120° C., and the setting speed is 8-10 m / min.

8. The production process of a high-flexibility polylactic acid fabric according to claim 4, characterized in that: The singeing temperature is 140°C.

Citation Information

Patent Citations

  • Corn fiber knitted fabric

    CN105040248A

  • Preparation method of halogen-free flame-retardant toughening polylactic acid composite material

    CN106832829A

  • Blended garment fabric

    CN110983583A

  • Knitted underwear fabric with moisture-absorbing, quick-drying and health-care functions and preparation method thereof

    CN113684601A

  • Preparation method of polylactic acid / polycaprolactone antibacterial blend fiber

    CN117328162A