Rapid lossless non-contact measuring device and measuring method for internal strain of silicon material

Through near-infrared femtosecond laser imaging technology, combined with time-domain stretching and spatial dispersion components, rapid lossless measurement of internal strain of silicon materials is achieved, solving the problems of speckle dependence and low frame rate in traditional methods, and achieving high efficiency and precision strain detection.

CN118913123AActive Publication Date: 2024-11-08WUHAN UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410898533.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-11-08
Estimated Expiration
2044-07-05

AI Technical Summary

Technical Problem

Traditional strain measurement methods rely on surface speckle production and low frame rate, making it difficult to meet the demand for fast lossless non-contact measurement of internal strain in silicon materials.

Method used

Using near-infrared femtosecond lasers, time-domain stretching components, optical signal amplification components, spatial dispersion components, microscopic objectives, high-speed photodetectors and data processing devices, the rapid internal strain of silicon materials is achieved through near-infrared femtosecond laser imaging. Lossless measurement avoids speckle production and high frame rate limits.

Benefits of technology

It realizes fast and accurate measurement of the internal strain of silicon material, and the frame rate reaches MHz level, reducing costs, avoiding sample damage and dependence on high frame rate equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118913123A_ABST
    Figure CN118913123A_ABST
Patent Text Reader

Abstract

The invention provides a rapid lossless non-contact measurement device and method for internal strain of a silicon material, and the device comprises a near-infrared femtosecond laser which is used for generating a near-infrared femtosecond laser pulse; the time domain stretching assembly is connected with the near-infrared femtosecond laser; the optical signal amplification assembly is connected with the time domain stretching assembly; the first space dispersion assembly is arranged on an emergent light path of the light signal amplification assembly; the microscope objective piece is arranged on an emergent light path of the spatial dispersion assembly; the second spatial dispersion assembly is arranged on an emergent light path of the microscope objective; the high-speed photoelectric detector is located on an emergent light path of the second spatial dispersion assembly; the high-speed oscilloscope is electrically connected with the high-speed photoelectric detector; and the data processing device is electrically connected with the high-speed oscilloscope and is used for processing and calculating the analog electric signal obtained by sampling to obtain the strain in the sample to be tested. The method is used for solving the problems of strong dependence on speckles and low detection frame number in the prior art.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of optical mechanics and deformation measurement, and in particular relates to a measurement method of a device for rapidly and non-destructively measuring the internal strain of silicon material without contact. Background Art

[0002] At present, the chip size has entered the nano era. Due to the reduction of chip packaging volume and the increase of chip overall power consumption, the heat generated by the chip is easy to accumulate, causing the chip temperature to rise. The chip substrate is often made of composite materials. Different components have different thermal expansion coefficients. Under temperature changes, thermal mismatch will occur inside, resulting in stress and strain, causing warping deformation, and even causing solder joint failure, chip cracking and delamination. Therefore, the detection of chip strain is receiving more and more attention.

[0003] Due to the small size of the chip and the microscopic measurement, the traditional contact strain measurement method based on strain gauges or extensometers is difficult to meet the needs of this field. At present, Digital Image Correlation (DIC) is a widely used non-contact measurement method in this field. This method first uses spraying, flooding, etching and other methods to make scattered spots on the surface of the sample, and then uses an optical microscope (OM) or a scanning electron microscope (SEM) to take the speckle image before and after deformation. By comparing the position changes of the scattered spots before and after deformation, the strain field distribution of the sample is analyzed and generated.

[0004] However, traditional strain measurement methods have two major limitations: First, traditional DIC technology is based on the production of speckles on the surface of the sample for analysis. The strain distribution and changes on the sample surface are calculated using an algorithm through the speckle patterns before and after deformation. The measurement quality depends largely on the quality of the speckle production. Second, traditional DIC technology requires expensive high-speed cameras to achieve high-frame-rate high-speed measurements. The frame rate is limited by the high-speed camera, with the maximum frame rate being in the order of 10,000 frames per second, and is constrained by the field of view size and resolution. Summary of the invention

[0005] One object of the present invention is to provide a device for fast, non-destructive and contactless measurement of internal strain of silicon materials in view of the shortcomings of the prior art, so as to solve the problems of the prior art's strong reliance on speckle and low detection frame number.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0007] A device for fast, non-destructive and non-contact measurement of internal strain of silicon material, comprising:

[0008] A near-infrared femtosecond laser, used to generate near-infrared femtosecond laser pulses that are sufficient to penetrate the sample to be tested for imaging without damaging the sample to be tested;

[0009] A time domain stretching component, connected to the near-infrared femtosecond laser, for performing time domain stretching on the near-infrared femtosecond laser pulse;

[0010] An optical signal amplifying component, which is connected to the time domain stretching component and is used to compensate the power of the near-infrared femtosecond laser pulse stretched by the time domain stretching component;

[0011] A first spatial dispersion component is arranged on the outgoing optical path of the optical signal amplification component and is used for spatially dispersing the outgoing near-infrared femtosecond laser pulse into spatial pulses;

[0012] A microscope objective lens component is arranged on the outgoing light path of the spatial dispersion component and is used to focus the spatial pulse onto the sample to be measured and transmit the spatial pulse focused on the sample to be measured;

[0013] A second spatial dispersion component is arranged on the outgoing light path of the microscope objective lens, and is used to converge the light pulses passing through the sample to be measured to obtain point light;

[0014] A high-speed photodetector, which is located on the outgoing light path of the second spatial dispersion component and is used to convert the transmitted light pulse signal into an analog signal;

[0015] A high-speed oscilloscope, electrically connected to the high-speed photodetector, for sampling analog electrical signals;

[0016] The data processing device is electrically connected to the high-speed oscilloscope and is used to process and calculate the sampled analog electrical signal to obtain the strain inside the sample to be tested.

[0017] Furthermore, it also includes an optical power meter. Before testing, the optical power meter is placed between the microscope objective lens and the sample to be tested. During testing, the optical power meter is moved out of the light path.

[0018] Furthermore, it also includes a first lens assembly and a second lens assembly, wherein the first lens assembly is arranged between the first spatial dispersion assembly and the microscope objective assembly, wherein the first lens assembly is used to adjust the size of the pulse spot and the angle of the pulse incident on the microscope objective assembly; the second lens assembly is arranged between the exit side of the sample to be tested and the second spatial dispersion assembly, and the second lens assembly is used to converge the transmitted pulse onto the second spatial dispersion assembly.

[0019] Furthermore, it also includes a first collimator and a second collimator, wherein the first collimator is located between the optical signal amplifying component and the first spatial dispersion component, and the first collimator is used to make the pulse amplified by the optical signal amplifying component incident on the first spatial dispersion component in the form of a specific angle and spatial light; the second collimator is located between the second spatial dispersion component and the high-speed photodetector, and the second collimator is used to couple the transmitted pulse into the optical path.

[0020] Furthermore, the first spatial dispersion component includes a first acousto-optic deflector and a first diffraction grating which are sequentially arranged on the output light path of the optical signal amplification component, the first acousto-optic deflector is used to change the propagation direction of the pulse to achieve the change of the incident position and angle of the femtosecond laser on the first diffraction grating, and the first diffraction grating is used to disperse the near-infrared femtosecond laser pulse into a one-dimensional spatial pulse.

[0021] Furthermore, the second spatial dispersion component includes a second diffraction grating and a second acousto-optic deflector which are sequentially arranged on the output light path of the microscope objective, the second diffraction grating is used to restore the one-dimensional spatial pulse to point light, and the second acousto-optic deflector is used to convert the two-dimensional scanning light beam passing through the sample into a one-dimensional spatial pulse.

[0022] Furthermore, the microscope objective lens component includes a first microscope objective lens and a second microscope objective lens which are sequentially arranged on the output light path of the first spatial dispersion component, and the sample to be measured is located on the light path between the first microscope objective lens and the second microscope objective lens.

[0023] Another object of the present invention is to provide a method for measuring the internal strain of silicon material according to the above-mentioned rapid non-destructive non-contact measuring device, comprising the following steps:

[0024] Step 1, clean the sample to be tested and fix it on the optical path of the microscope objective lens;

[0025] Step 2, starting the near-infrared femtosecond laser to generate near-infrared femtosecond laser pulses that are sufficient to penetrate the sample to be tested for imaging without damaging the sample to be tested;

[0026] Step 3: The time domain stretching component performs time domain stretching on the near-infrared femtosecond pulse, amplifies the pulse through the optical signal amplification component, and then focuses the pulse onto the sample to be tested through the first spatial dispersion component and the microscope objective lens component;

[0027] Step 4. The pulse passing through the sample to be tested is incident on a high-speed photodetector and a high-speed oscilloscope in sequence through a second spatial dispersion component, and is finally transmitted to a data processing device. The data processing device restores a distribution image sequence of the light pulse signal transmitted through the sample to be tested according to the analog electrical signal sampled by the high-speed oscilloscope, obtains the change in the contour boundary of the light intensity distribution image before and after the sample to be tested is strained according to the light pulse signal distribution image sequence, calculates the strain of each area, and finally obtains the strain inside the sample to be tested by interpolation calculation.

[0028] Furthermore, the method for obtaining a light intensity distribution image sequence includes:

[0029] Construct a two-dimensional light intensity distribution image sequence transmitted through the sample to be tested, whose frame rate is equal to the repetition frequency of the near-infrared femtosecond laser, from the sampled light pulse signal I(x) to the light intensity signal I s The conversion formula of (x) is as follows:

[0030]

[0031] Among them, I R (x) is the reference pulse intensity, T is the Hilbert transformed component of the filtered high-frequency component of the sampled optical pulse signal I(x), and re(T) and im(T) are the real part and imaginary part of T, respectively.

[0032] Furthermore, the method for the data processing device to calculate the internal strain of the sample to be tested according to the optical pulse signal distribution image sequence includes:

[0033] The light intensity distribution image sequence is filtered using the non-local mean algorithm, and then a binary image is extracted from the filtered light intensity distribution image sequence. The eigenvalue and eigenvector method is used to track the distribution of each contour area of ​​the sample before and after strain. The position coordinate matrix A of each contour area at the boundary of the sample to be tested is expressed as: A = QΛQ, where Q is the matrix of eigenvectors and Λ is the matrix of eigenvalues;

[0034] The deformation of each contour area before and after strain is expressed as:

[0035]

[0036] Where: e i is a unit vector; and Represents the transformation matrix of each contour area before and after strain; E j is the characteristic value of the region;

[0037] The deformation tensor It is expressed as:

[0038]

[0039] Strain in each contour area Calculated by the following formula:

[0040]

[0041] Compared with the prior art, the present invention has the following beneficial effects: the present invention uses near-infrared light to perform ultrafast laser imaging on the sample to be tested, and the imaging frame rate is equivalent to the pulse repetition frequency of the laser, which can reach about MHz, so that the strain of the silicon material can be quickly measured; in addition, due to the penetration of near-infrared light into silicon materials, the image sequence formed by the method of the present invention contains the structural information inside the chip or device to be tested, and after the image sequence is processed by a data processing device, the strain change inside the chip or device to be tested can be accurately reflected, so that the strain information obtained is relatively accurate;

[0042] Compared with the non-contact traditional DIC technology, the present invention overcomes the difficulty of DIC technology requiring the preparation of speckles, and uses images derived from the structural characteristics of the sample chip itself for calculation and analysis, without the need to additionally produce speckles on the sample, thereby avoiding damage to the sample surface; by controlling the laser power, the generated laser of a specific wavelength can have a specific power after amplification, so that the laser does not damage the sample while passing through the sample and forming the image required for the test, thereby realizing non-contact non-destructive testing;

[0043] In addition, the present invention does not require expensive high-speed cameras and is not constrained by frame rate, field of view size and resolution. It only requires commonly used near-infrared femtosecond lasers to quickly measure the strain changes inside the chip or device to be tested, greatly reducing costs and improving measurement efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 This is a schematic structural diagram of a device for rapid, non-destructive, and contactless measurement of internal strain of silicon material provided in Example 1 of the present invention. DETAILED DESCRIPTION

[0045] The technical solutions in the embodiments of the present invention will be described clearly and completely below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0046] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.

[0047] The present invention will be further described below in conjunction with specific embodiments, but the present invention is not limited thereto.

[0048] Embodiment 1:

[0049] Embodiment 1 provides a device for ultrafast non-destructive and non-contact measurement of internal strain of silicon material, such as Figure 1 As shown, it includes: a near-infrared femtosecond laser 101, a time-domain stretching component, an optical signal amplifying component, a first spatial dispersion component, a microscope objective lens component, a second spatial dispersion component, a high-speed photodetector, a high-speed oscilloscope, and a data processing device. In this embodiment, the time-domain stretching component is a single-mode optical fiber 102, which is arranged on the output optical path of the near-infrared femtosecond laser 101; the optical signal amplifying component is an erbium-doped fiber amplifier 103, which is arranged on the output optical path of the single-mode optical fiber 102. In order to allow the pulse amplified by the erbium-doped fiber amplifier 103 to be incident on the first spatial dispersion component at a specific angle and in the form of spatial light, a first collimator 104 is also arranged on the optical path between the erbium-doped fiber amplifier 103 and the first spatial dispersion component.

[0050] The first spatial dispersion component includes a first acousto-optic deflector 105 and a first diffraction grating 106 which are sequentially arranged on the output light path of the first collimator 104, wherein the first acousto-optic deflector 105 is used to change the propagation direction of the near-infrared femtosecond laser pulse to achieve the change of the incident position and angle of the femtosecond laser on the first diffraction grating 106, and the first diffraction grating 106 is used to disperse the near-infrared femtosecond laser pulse into a one-dimensional spatial pulse. In this embodiment, the microscope objective component includes a first microscope objective 109 and a second microscope objective 111 which are sequentially arranged on the output light path of the first diffraction grating 106, wherein the sample to be measured is arranged on the light path between the first microscope objective 109 and the second microscope objective 111. In order to ensure that the pulse generated by the near-infrared femtosecond laser 101 has a first power and a first wavelength after being amplified by the erbium-doped fiber amplifier 103, the first power is sufficient to penetrate the sample to be tested without damaging the object to be tested, and the first wavelength is sufficient to form an image with sufficient quality after penetrating the silicon and other polymer components of the sample to be tested, before the test, an optical power meter 110 is set between the first microscope objective lens 109 and the sample to be tested, and the optical power meter 110 is moved out of the light path after the test starts.

[0051] In addition, a first lens assembly and a second lens assembly are provided, wherein the first lens assembly includes a first plano-convex lens 107 and a second plano-convex lens 108 sequentially arranged on the optical path between the first spatial dispersion assembly and the microscope objective, wherein the first lens assembly is used to adjust the size of the pulse spot and the angle at which the pulse is incident on the microscope objective. The second lens assembly includes a third plano-convex lens 112 and a fourth plano-convex lens 113 sequentially arranged on the optical path between the second microscope objective and the second spatial dispersion assembly, and the second lens assembly is used to converge the transmission pulse onto the second spatial dispersion assembly.

[0052] The second spatial dispersion component includes a second diffraction grating 114 and a second acousto-optic deflector 115 which are sequentially arranged on the exit side of the fourth plano-convex lens 113. The second diffraction grating 114 is used to restore the one-dimensional spatial pulse to a point light, and the second acousto-optic deflector 115 is used to convert the two-dimensional scanning light beam passing through the sample to be tested into a one-dimensional spatial pulse. Among them, the first plano-convex lens 107, the second plano-convex lens 108, the first microscope objective lens 109, the sample to be tested, the second microscope objective lens 111, the third plano-convex lens 112, and the fourth plano-convex lens 113 are located on the same optical axis.

[0053] The high-speed photodetector 117 is arranged on the outgoing optical path of the second acousto-optic deflector 115, and is used to convert the transmitted light pulse signal into an analog signal. In this embodiment, the high-speed photodetector 117 selects the MHz-level and above high-speed free-space photodetector 117. In order to facilitate coupling the transmitted pulse into the optical path for detection by the high-speed photodetector 117, a second collimator 116 is arranged between the second acousto-optic deflector 115 and the high-speed photodetector 117. A high-speed oscilloscope 118 for sampling analog electrical signals is electrically connected to the downstream of the high-speed photodetector 117. In this embodiment, the high-speed oscilloscope selects a MHz-level and above high-speed oscilloscope. The data processing device 119 is electrically connected to the high-speed oscilloscope 118, and is used to restore the distribution image sequence of the light pulse signal transmitted through the sample to be tested according to the sampled analog electrical signal; and obtain the change of the contour boundary of the light intensity distribution image before and after the strain of the object to be tested according to the light signal image sequence, calculate the boundary strain, and obtain the strain inside the sample to be tested by interpolation calculation. In this embodiment, the data processing device 119 is a computer or other equipment capable of data processing and calculation.

[0054] Embodiment 2:

[0055] Embodiment 2 provides an ultrafast, non-destructive, and non-contact measurement method for the internal strain of a silicon material, which is implemented using the device provided in Embodiment 1 and mainly includes the following steps:

[0056] Step 1: clean and dry the sample to be tested using chemical detergent and deionized water, and fix it on the optical path between the first microscope objective lens 109 and the second microscope objective lens 111;

[0057] Step 2: Before the test, the optical power meter 110 is set on the optical path between the first microscope objective lens 109 and the sample to be tested, and the near-infrared femtosecond laser 101 and the erbium-doped fiber amplifier 103 are adjusted so that the femtosecond laser pulse generated by the near-infrared femtosecond laser 101 has a first power and a first wavelength after being amplified by the erbium-doped fiber amplifier 103, and the first power is sufficient to penetrate the sample to be tested without damaging the sample to be tested, and the first wavelength is sufficient to form an image with sufficient quality after penetrating the silicon and other polymer components of the sample to be tested; after the test starts, the optical power meter 110 is moved out of the optical path, and the pulse power and wavelength emitted and amplified by the near-infrared femtosecond laser 101 and the erbium-doped fiber amplifier 103 are kept unchanged;

[0058] Step 3: Time-domain stretching of near-infrared femtosecond laser pulses is performed through the single-mode optical fiber 102, and the pulses after time-domain stretching are incident on the first acousto-optic deflector 105 at a specific angle and in the form of spatial light through the first collimator 104; the refractive properties of the crystal inside the acousto-optic deflector are changed by controlling the acoustic wave driving frequency, thereby realizing the change of the incident position and angle of the femtosecond laser on the first diffraction grating 106;

[0059] Step 4: The spatial light incident on the first diffraction grating 106 at different positions and angles is dispersed into one-dimensional spatial pulses, and then focused on different positions on the sample to be measured through the first plano-convex lens 107, the second plano-convex lens 108, and the first microscope objective lens 109, thereby realizing a large-scale two-dimensional scanning of the one-dimensional femtosecond laser on the object to be measured;

[0060] Step 5, the pulse passing through the sample to be tested passes through the second microscope objective 111, the third plano-convex lens 112, and the fourth plano-convex lens 113, and passes through the second diffraction grating 114 and the second acousto-optic deflector 115 at an angle opposite to that of the incident angle, and is re-shaped into a one-dimensional pulse and coupled to the MHz-level and above high-speed photodetector 117 through the second collimator 116, thereby converting the transmitted light pulse signal into an analog signal;

[0061] Step 6: The transmitted pulse is converted into an analog electrical signal after passing through the high-speed photodetector 117, and then sampled to the computer 119 through the high-speed oscilloscope 118. The computer 119 analyzes and reconstructs the analog signal sampled by the high-speed oscilloscope 118 to obtain a two-dimensional light intensity distribution diagram sequence, whose frame rate is equal to the repetition frequency of the near-infrared femtosecond laser, from the sampled light pulse signal I(x) to the light intensity signal I s The conversion formula of (x) is as follows:

[0062]

[0063] Among them, I R(x) is the reference pulse intensity, T is the Hilbert transformed component of the filtered high-frequency component of the sampled optical pulse signal I(x), and re(T) and im(T) are the real part and imaginary part of T, respectively.

[0064] For the light intensity distribution image sequence obtained by the above formula, in order to reduce the influence of test noise such as photodetector noise and oscilloscope measurement noise on the measurement results, the non-local mean algorithm is used for filtering to clarify the boundaries of each contour area in the image. The calculation formula of the algorithm is:

[0065] NL[v](i)=∑ j∈I v(j)w(i,j) (2)

[0066] Where NL[v](i) is the filtered image of pixel i, v(j) is the original image without filtering; I is the neighborhood of pixel i; w(i,j) represents the similarity between pixels i and j, and its value is determined by the square of the Euclidean distance between the search windows:

[0067]

[0068] in,

[0069]

[0070] In the formula, h is a smoothing parameter that controls the attenuation degree of the Gaussian function, and its specific value is based on the image noise level; is the attenuation function of the weighted Euclidean distance between pixel i and pixel j, a is the standard deviation of the Gaussian kernel; Z i is the normalization coefficient.

[0071] After filtering the light intensity distribution image sequence, the binary image is extracted, and the eigenvalue and eigenvector method is used to track the contour area distribution of the object to be measured before and after strain. The position coordinate matrix A of each area to the sample boundary can be expressed as A=QΛQ, where Q is the matrix of eigenvectors and Λ is the matrix of eigenvalues. The deformation of each area before and after strain can be expressed as:

[0072]

[0073] Where: e i is a unit vector; and Represent the transformation matrix of the area before and after strain respectively; E j is the eigenvalue of the region. Then the deformation tensor It can be expressed as:

[0074]

[0075] Strain in each region It can be calculated by the following formula:

[0076]

[0077] Get the strain of each area Afterwards, the node matrix is ​​constructed with the strains in each area and imported into MATLAB to call the two-dimensional spline interpolation toolbox. The strain distribution at various locations inside the measured sample can be obtained through interpolation calculation.

[0078] Example 2 utilizes the characteristics of near-infrared femtosecond laser pulse waves that are at the femtosecond level and can penetrate silicon materials, and uses diffraction gratings and acousto-optic deflectors to form spatial pulse dispersion into spatial pulses that scan the surface of the object to be measured in two dimensions, thereby ultra-fast acquisition of the light intensity distribution of the pulse after passing through the object to be measured, and the strain distribution inside the object to be measured can be calculated with the algorithm. The entire measurement process is contactless, and can achieve ultra-fast, non-destructive, non-contact strain measurement of the observed object, and can measure the strain distribution inside the object to be measured, with a sampling frequency of up to 10 6 Hz and above, it can effectively observe the transient strain distribution inside electronic chips or devices.

[0079] The above are only preferred embodiments of the present invention, and are not intended to limit the implementation methods and protection scope of the present invention. Those skilled in the art should be aware that all solutions obtained by equivalent substitutions and obvious changes made using the contents of the specification of the present invention should be included in the protection scope of the present invention.

Claims

1. A device for fast, non-destructive and non-contact measurement of internal strain of silicon material, characterized in that: include: A near-infrared femtosecond laser, used to generate near-infrared femtosecond laser pulses that are sufficient to penetrate the sample to be tested for imaging without damaging the sample to be tested; A time domain stretching component is arranged on the output optical path of the near-infrared femtosecond laser and is used for time domain stretching the near-infrared femtosecond laser pulse; An optical signal amplifying component, which is arranged in connection with the outgoing optical path of the time domain stretching component and is used for power compensation of the near-infrared femtosecond laser pulse stretched by the time domain stretching component; A first spatial dispersion component is arranged on the outgoing optical path of the optical signal amplification component and is used for spatially dispersing the outgoing near-infrared femtosecond laser pulse into spatial pulses; A microscope objective lens component, which is arranged on the outgoing light path of the first spatial dispersion component and is used to focus the spatial pulse onto the sample to be measured and transmit the spatial pulse focused on the sample to be measured; A second spatial dispersion component is arranged on the outgoing light path of the microscope objective lens, and is used to converge the light pulses passing through the sample to be measured to obtain point light; A high-speed photodetector, which is located on the outgoing light path of the second spatial dispersion component and is used to convert the transmitted light pulse signal into an analog signal; A high-speed oscilloscope, electrically connected to the high-speed photodetector, for sampling analog electrical signals; The data processing device is electrically connected to the high-speed oscilloscope and is used to process and calculate the sampled analog electrical signal to obtain the strain inside the sample to be tested.

2. The device for rapid, non-destructive, and non-contact measurement of internal strain of silicon materials according to claim 1, characterized in that: It also includes an optical power meter. Before testing, the optical power meter is placed between the microscope objective lens and the sample to be tested. During testing, the optical power meter is moved out of the light path.

3. The device for rapid, non-destructive, and non-contact measurement of internal strain of silicon material according to claim 1, characterized in that: It also includes a first lens assembly and a second lens assembly, wherein the first lens assembly is arranged between the first spatial dispersion assembly and the microscope objective assembly, wherein the first lens assembly is used to adjust the size of the pulse spot and the angle at which the pulse is incident on the microscope objective assembly; and the second lens assembly is arranged between the exit side of the sample to be measured and the second spatial dispersion assembly, wherein the second lens assembly is used to converge the transmitted pulse onto the second spatial dispersion assembly.

4. The device for rapid, non-destructive, and non-contact measurement of internal strain of silicon material according to claim 1, characterized in that: It also includes a first collimator and a second collimator, wherein the first collimator is located between the optical signal amplifying component and the first spatial dispersion component, and is used to make the pulse amplified by the optical signal amplifying component incident on the first spatial dispersion component in the form of a specific angle and spatial light; the second collimator is located between the second spatial dispersion component and the high-speed photodetector, and is used to couple the transmitted pulse into the optical path.

5. The device for rapid, non-destructive, and non-contact measurement of internal strain of silicon material according to claim 1, characterized in that: The first spatial dispersion component includes a first acousto-optic deflector and a first diffraction grating which are sequentially arranged on the output light path of the optical signal amplification component, wherein the first acousto-optic deflector is used to change the propagation direction of the pulse, and the first diffraction grating is used to disperse the near-infrared femtosecond laser pulse into a one-dimensional spatial pulse.

6. The ultrafast non-destructive non-contact measurement device for internal strain of silicon material according to claim 1, characterized in that: The second spatial dispersion component includes a second diffraction grating and a second acousto-optic deflector which are sequentially arranged on the output light path of the microscope objective, the second diffraction grating is used to restore the one-dimensional spatial pulse to point light, and the second acousto-optic deflector is used to convert the two-dimensional scanning light beam passing through the sample into a one-dimensional spatial pulse.

7. The device for rapid, non-destructive, and non-contact measurement of internal strain of silicon material according to claim 1, characterized in that: The microscope objective lens component comprises a first microscope objective lens and a second microscope objective lens which are sequentially arranged on the outgoing light path of the first spatial dispersion component, and the sample to be measured is located on the light path between the first microscope objective lens and the second microscope objective lens.

8. A method for measuring the internal strain of silicon material according to any one of claims 1 to 7, characterized in that: The steps include: Step 1, clean the sample to be tested and fix it on the optical path of the microscope objective lens; Step 2, starting the near-infrared femtosecond laser to generate near-infrared femtosecond laser pulses that are sufficient to penetrate the sample to be tested for imaging without damaging the sample to be tested; Step 3: The time domain stretching component performs time domain stretching on the near-infrared femtosecond pulse, amplifies the pulse through the optical signal amplification component, and then focuses the pulse onto the sample to be tested through the first spatial dispersion component and the microscope objective lens component; Step 4. The pulse passing through the sample to be tested is incident on a high-speed photodetector and a high-speed oscilloscope in sequence through a second spatial dispersion component, and is finally transmitted to a data processing device. The data processing device restores a distribution image sequence of the light pulse signal transmitted through the sample to be tested based on the analog electrical signal sampled by the high-speed oscilloscope, obtains the change in the contour area of ​​the light intensity distribution image before and after the sample to be tested is strained based on the light pulse signal distribution image sequence, calculates the strain in each area, and finally obtains the strain inside the sample to be tested through interpolation calculation.

9. The method for measuring the internal strain of silicon material according to claim 8, characterized in that: The method of obtaining a light intensity distribution image sequence includes: Construct a two-dimensional light intensity distribution image sequence transmitted through the sample to be tested, whose frame rate is equal to the repetition frequency of the near-infrared femtosecond laser, from the sampled light pulse signal I(x) to the light intensity signal I s The conversion formula of (x) is as follows: Among them, I R (x) is the reference pulse intensity, T is the Hilbert transformed component of the filtered high-frequency component of the sampled optical pulse signal I(x), and re(T) and im(T) are the real part and imaginary part of T, respectively.

10. The method for measuring the internal strain of silicon material according to claim 8, characterized in that: The method for calculating the internal strain of the sample to be tested according to the optical pulse signal distribution image sequence by the data processing device comprises: The light intensity distribution image sequence is filtered using the non-local mean algorithm, and then a binary image is extracted from the filtered light intensity distribution image sequence. The eigenvalue and eigenvector method is used to track the distribution of each contour area of ​​the sample before and after strain. The position coordinate matrix A of each area at the boundary of the sample to be tested is expressed as: A = QΛQ, where Q is the matrix of eigenvectors and Λ is the matrix of eigenvalues; The deformation of each region before and after strain is expressed as: Where: e i is a unit vector; and Represents the transformation matrix of each contour area before and after strain; E j is the characteristic value of the region; The deformation tensor It is expressed as: Strain in each region Calculated by the following formula:

Citation Information

Patent Citations

  • Single-pixel high-speed super-resolution imaging device and method based on time domain stretching

    CN109100304A

  • Large-aperture optical element high-speed detection system based on ultrafast microscopic imaging

    CN113624453A

  • Ultrafast temperature measuring device and method for light-transmitting object based on femtosecond laser

    CN115014569A

  • Rapid lossless non-contact measuring device and measuring method for surface strain of silicon material

    CN118913122A

  • Silicon wafer stress lossless non-contact measurement method and device

    CN120651401A