Method for removing large-size residual defects on photoetching mask plate

By covering the photoresist on the photolithography mask and using laser irradiation to high temperature vaporization, the etching window is formed and the chromium residual defects are removed by using etching liquid to remove chromium residual defects in the prior art. The waste caused by large-size chromium residual defects in the prior art is solved and The cost increase problem has achieved efficient and defect-free repair results.

CN118915380APending Publication Date: 2024-11-08TOPPAN PHOTOMASKS COMPANY LIMITED
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310500486.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-06
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art often leads to waste and increase in plate making costs when dealing with large-size chromium residue defects on lithography masks, especially lasers produce residues, and ion beam or electron beam etching time is too long, resulting in the choice of re-made rather than repair.

Method used

By covering the photoresist on the photolithography mask, using laser irradiation to remove the photoresist in the residual defect area, forming an etching window, and then using etching liquid to remove residual defects, achieving defect-free residue and short process time Effect.

Benefits of technology

Effectively removes large-size chromium residual defects, avoids waste of masks, significantly saves manufacturing costs, and ensures efficient process and defect-free residues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118915380A_ABST
    Figure CN118915380A_ABST
Patent Text Reader

Abstract

The invention provides a method for removing a large-size residual defect on a photoetching mask plate, which comprises the following steps: 1) providing the photoetching mask plate which has a shading material residual defect, and the maximum radial size of the shading material residual defect is greater than or equal to 50 microns; (2) the photoetching mask plate is covered with photoresist; (3) irradiating the photoresist in the residual defect area of the shading material through laser, and removing the photoresist in the area in a high-temperature gasification manner to form an etching window for exposing the residual defect of the shading material; 4) removing the residual defect of the shading material in the etching window through etching liquid; and 5) removing the photoresist. The method has the advantages of being free of defect residues and short in process time, and meanwhile, waste of the photoetching mask plate can be avoided, so that the manufacturing cost is greatly saved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of semiconductor integrated circuit manufacturing, and in particular relates to a method for removing large-size residual defects on a photolithography mask. Background Art

[0002] During the manufacturing process of the mask, various defects will occur due to various reasons. Common defects include chrome spots, pinhole chrome protrusions, chrome missing, etc. These defects will cause a large number of wafers to be scrapped during use. Therefore, in order to ensure the yield of the mask during use in the wafer factory, the wafer factory requires the defects to be repaired before the mask is shipped. At present, in the mask manufacturing industry, for chromium residual defects, using lasers to generate high temperatures to vaporize the defects and using focused ion beams or electron beams to etch are relatively common repair methods. However, no matter which of the above methods is used, when encountering defects of larger size, difficulties will be encountered. For example, laser lasers will produce a large amount of residues, while using ion beams or electron beams will encounter the problem of too long repair time. In the current repair technology, when encountering large-sized chromium residual defects, it is usually chosen not to repair the mask, but to directly remake a new mask, which will lead to a great degree of waste, and remaking the plate will greatly increase the cost.

[0003] It should be noted that the above introduction to the technical background is only for the convenience of providing a clear and complete description of the technical solutions of the present application and for the convenience of understanding by those skilled in the art. It cannot be considered that the above technical solutions are well known to those skilled in the art simply because they are described in the background technology section of the present application. Summary of the invention

[0004] In view of the above-mentioned shortcomings of the prior art, an object of the present invention is to provide a method for removing large-sized residual defects on a photolithography mask, so as to solve the problem in the prior art that large-sized residual defects lead to mask waste and increased plate making costs.

[0005] To achieve the above-mentioned purpose and other related purposes, the present invention provides a method for removing large-sized residual defects on a photolithography mask, the removal method comprising the following steps: 1) providing a photolithography mask, the photolithography mask having residual defects of shading material, the maximum radial size of the residual defects of shading material being greater than or equal to 50 microns; 2) covering the photolithography mask with photoresist; 3) irradiating the photoresist in the area of ​​the residual defects of shading material with a laser to remove the photoresist in the area by high-temperature vaporization to form an etching window revealing the residual defects of shading material; 4) removing the residual defects of shading material in the etching window by an etching solution; 5) removing the photoresist.

[0006] Optionally, the photolithography mask includes a light-transmitting area and a light-shielding area, and the light-shielding material residual defect is located in the light-transmitting area.

[0007] Optionally, there is a gap between a boundary of the residual defect of the light-shielding material and a boundary of the light-shielding area.

[0008] Optionally, the etching window reveals the boundary of the residual defect of the light-shielding material and completely covers the boundary of the light-shielding area.

[0009] Optionally, the maximum radial size of the residual defects of the shading material is 50 microns to 200 microns.

[0010] Optionally, the light-shielding material includes chromium or a chromium compound.

[0011] Optionally, the substrate of the photolithography mask includes a quartz substrate.

[0012] Optionally, in step 2), the photolithography mask is covered with photoresist by spin coating, and the thickness of the photoresist is controlled to be 300 nanometers to 350 nanometers.

[0013] Optionally, the wavelength of the laser in step 3) is 248 nanometers.

[0014] Optionally, in step 5), the photoresist is removed by an SPM cleaning method, wherein the cleaning solution used in the SPM cleaning method comprises H 2 SO 4 Solution and H 2 O 2 Mixed solution of solution preparation.

[0015] As described above, the method for removing large-size residual defects on a photolithography mask of the present invention has the following beneficial effects:

[0016] The invention provides a method for removing large-size (e.g., 50 to 200 microns) chromium residual defects in a fully transparent area, by covering a photoresist on a photolithography mask, irradiating the photoresist in the area of ​​residual defects of a shading material by laser, and removing the photoresist in the area by high-temperature vaporization to form an etching window that reveals the residual defects of the shading material, and then removing the residual defects of the shading material in the etching window by an etching liquid to eliminate the defects of the photolithography mask. The invention has the advantages of no defect residue and short process time, and can avoid the waste of photolithography masks, thereby greatly saving manufacturing costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The included drawings are used to provide a further understanding of the embodiments of the present application, which constitute a part of the specification, are used to illustrate the implementation of the present application, and together with the text description, explain the principles of the present application. Obviously, the drawings described below are only some embodiments of the present application.

[0018] Figure 1 to Figure 7 It is a schematic structural diagram showing the steps of a method for removing large-sized residual defects on a photolithography mask according to an embodiment of the present invention.

[0019] Component number description

[0020] 10 Photolithography Mask

[0021] 101 Quartz substrate

[0022] 102 Shading area

[0023] 103 Residual defects of shading material

[0024] 104 Photoresist

[0025] 105 Laser

[0026] 106 Etching Window DETAILED DESCRIPTION

[0027] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0028] It should be emphasized that the term “include / comprises” when used herein refers to the presence of features, integers, steps or components, but does not exclude the presence or addition of one or more other features, integers, steps or components.

[0029] Features described and / or illustrated with respect to one embodiment may be used in the same or similar manner in one or more other embodiments, combined with features in other embodiments, or substituted for features in other embodiments.

[0030] For example, when describing the embodiments of the present invention in detail, for the sake of convenience, the cross-sectional view showing the device structure will not be partially enlarged according to the general scale, and the schematic view is only an example, which should not limit the scope of protection of the present invention. In addition, in actual production, the three-dimensional space dimensions of length, width and depth should be included.

[0031] For ease of description, spatially relative terms such as "under", "below", "below", "below", "above", "on", etc. may be used herein to describe the relationship of one element or feature shown in the drawings to other elements or features. It will be understood that these spatially relative terms are intended to encompass other orientations of the device in use or operation in addition to the orientation depicted in the drawings. In addition, when a layer is referred to as being "between" two layers, it can be the only layer between the two layers, or one or more intervening layers may also be present.

[0032] In the context of the present application, a structure in which a first feature is described as being "above" a second feature may include embodiments in which the first and second features are formed in direct contact, and may also include embodiments in which additional features are formed between the first and second features, such that the first and second features may not be in direct contact.

[0033] It should be noted that the illustrations provided in this embodiment are only used to illustrate the basic concept of the present invention in a schematic manner, and therefore the illustrations only show components related to the present invention rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.

[0034] like Figure 1 to Figure 7 As shown, the present invention provides a method for removing large-size residual defects on a photolithography mask, and the removal method comprises the following steps:

[0035] like Figure 1 As shown, firstly, step 1) is performed to provide a photolithography mask 10, on which there are light-shielding material residual defects 103, and the maximum radial size of the light-shielding material residual defects 103 is greater than or equal to 50 microns.

[0036] In one embodiment, the substrate of the photolithography mask 10 includes a quartz substrate 101 , and the transmittance of the quartz substrate 101 to exposure light is greater than 80%.

[0037] In one embodiment, the photolithography mask 10 includes a light-transmitting area and a light-shielding area 102 , and the light-shielding material residual defect 103 is located in the light-transmitting area.

[0038] In one embodiment, Figure 1 As shown, there is a gap between the boundary of the light shielding material residual defect 103 and the boundary of the light shielding region 102. For example, the gap between the boundary of the light shielding material residual defect 103 and the boundary of the light shielding region 102 may be 10 to 100 micrometers, but is not limited to the examples listed here.

[0039] In one embodiment, the maximum radial dimension of the residual defect 103 of the shading material is 50 microns to 200 microns, and the radial dimension of the light-transmitting area is greater than the maximum radial dimension of the residual defect 103 of the shading material. For example, in one embodiment, the maximum radial dimension of the residual defect 103 of the shading material is 80 microns, and the radial dimension of the light-transmitting area is 120 microns. When the residual defect 103 of the shading material is located in the middle of the light-transmitting area, the boundary of the residual defect 103 of the shading material is about 20 microns from the boundary of the light-transmitting area. Of course, the residual defect 103 of the shading material can also be offset from the middle of the light-transmitting area to a certain extent, such as the gaps between the two opposite boundaries of the shading material and the light-transmitting area can be about 10 microns and 30 microns respectively, and it is not limited to the examples listed here.

[0040] In one embodiment, the light shielding material includes chromium or a chromium compound. In a specific example, the light shielding material is chromium.

[0041] like Figure 2 As shown, step 2) is then performed to cover the photolithography mask 10 with a photoresist 104 .

[0042] In one embodiment, in step 2), the photoresist 104 is covered on the photolithography mask 10 by spin coating, and the thickness of the photoresist 104 is controlled to be between 300 nanometers and 350 nanometers. In a specific example, the photoresist 104 is IP3500 photoresist.

[0043] In one embodiment, after the photoresist 104 is spin-coated, a step of baking the photoresist 104 to improve its structural strength is also included.

[0044] like Figure 3-4 As shown, then step 3) is performed, the photoresist 104 in the area of ​​the residual defect 103 of the shading material is irradiated by the laser 105 to remove the photoresist 104 in the area by high-temperature gasification, so as to form an etching window 106 that reveals the residual defect 103 of the shading material;

[0045] In one embodiment, the wavelength of the laser 105 in step 3) is 248 nanometers. In this example, the method of removing the photoresist 104 by high-temperature vaporization through irradiation with the laser 105 can greatly save process costs and equipment costs compared to the exposure and development process, and it only requires a shorter process time and has a higher processing efficiency.

[0046] In one embodiment, the etching window 106 reveals the boundary of the light-shielding material residual defect 103 and completely covers the boundary of the light-shielding region 102. For example, the edge of the etching window 106 can be set to exceed the boundary of the light-shielding region 102 as much as possible and be close to the boundary of the light-shielding material residual defect 103 region, such as the edge of the etching window 106 can be set to be no more than 1 to 2 microns from the boundary of the light-shielding material residual defect 103 region. On the one hand, the light-shielding region 102 can be more fully protected, and on the other hand, more of the quartz substrate surface between the light-shielding region 102 and the light-shielding material residual defect 103 region can be covered, thereby avoiding the influence of the subsequent etching solution on the quartz substrate.

[0047] like Figure 5-6 As shown, step 4 is then performed to remove the residual defects 103 of the light shielding material in the etching window 106 by etching solution.

[0048] In one embodiment, the residual defect 103 of the light-shielding material is chromium, which can be removed by etching the residual defect of chromium with an etching solution composed of ammonium cerium nitrate, aqueous nitric acid solution and water. The etching rate of the etching solution on the quartz substrate 101 is very low, so when removing the residual defect of chromium, it is possible to avoid causing defects to the quartz substrate 101. In one embodiment, in order to improve the removal efficiency of the residual defect of chromium, a cationic surfactant can also be added to the etching solution.

[0049] In one embodiment, the etching temperature may be room temperature (about 25 degrees Celsius), and the etching time may be 15 to 120 seconds, depending on the complete removal of the chromium residual defects.

[0050] like Figure 7 As shown, step 5) is finally performed to remove the photoresist 104 to obtain a photolithography mask 10 without residual defects.

[0051] In one embodiment, step 5) removes the photoresist 104 by an SPM cleaning method, wherein the cleaning solution used in the SPM cleaning method includes H 2 SO 4 Solution and H 2 O 2 Mixed solution of solution preparation.

[0052] As described above, the method for removing large-size residual defects on a photolithography mask of the present invention has the following beneficial effects:

[0053] The invention provides a method for removing large-size (e.g., 50 to 200 microns) chromium residual defects in a fully transparent area, by covering a photoresist on a photolithography mask, irradiating the photoresist in the residual defect area of ​​the shading material with a laser, and removing the photoresist in the area by high-temperature vaporization to form an etching window that reveals the residual defect of the shading material, and then removing the residual defect of the shading material in the etching window with an etching liquid, thereby eliminating the defects of the photolithography mask. The invention has the advantages of no defect residue and short process time, and can avoid the waste of the photolithography mask, thereby greatly saving manufacturing costs.

[0054] Therefore, the present invention effectively overcomes various shortcomings in the prior art and has high industrial utilization value.

[0055] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A method for removing large-size residual defects on a photolithography mask, characterized in that: The removal method comprises the following steps: 1) providing a photolithography mask having a residual light-shielding material defect on the photolithography mask, wherein the maximum radial dimension of the residual light-shielding material defect is greater than or equal to 50 micrometers; 2) covering the photolithography mask with photoresist; 3) irradiating the photoresist in the residual defect area of ​​the light-shielding material with a laser to remove the photoresist in the area by high-temperature gasification, so as to form an etching window that reveals the residual defect of the light-shielding material; 4) removing residual defects of the light-shielding material in the etching window by etching liquid; 5) Removing the photoresist.

2. The method for removing large-size residual defects on a photolithography mask according to claim 1, characterized in that: The photolithography mask comprises a light-transmitting area and a light-shielding area, and the light-shielding material residual defect is located in the light-transmitting area.

3. The method for removing large-size residual defects on a photolithography mask according to claim 2, characterized in that: There is a gap between a boundary of the light shielding material residual defect and a boundary of the light shielding area.

4. The method for removing large-size residual defects on a photolithography mask according to claim 3, characterized in that: The etching window reveals the boundary of the residual defect of the light-shielding material and completely covers the boundary of the light-shielding area.

5. The method for removing large-size residual defects on a photolithography mask according to claim 1, characterized in that: The maximum radial size of the residual defects of the shading material is 50 microns to 200 microns.

6. The method for removing large-size residual defects on a photolithography mask according to claim 1, characterized in that: The light shielding material includes chromium or a chromium compound.

7. The method for removing large-size residual defects on a photolithography mask according to claim 1, characterized in that: The substrate of the photolithography mask plate includes a quartz substrate.

8. The method for removing large-size residual defects on a photolithography mask according to claim 1, characterized in that: Step 2) Covering the photolithography mask with photoresist by spin coating, wherein the thickness of the photoresist is controlled to be between 300 nanometers and 350 nanometers.

9. The method for removing large-size residual defects on a photolithography mask according to claim 1, characterized in that: Step 3) The wavelength of the laser is 248 nanometers.

10. The method for removing large-size residual defects on a photolithography mask according to claim 1, characterized in that: Step 5) removing the photoresist by an SPM cleaning method, wherein the cleaning solution used in the SPM cleaning method includes a mixed solution of H2SO4 solution and H2O2 solution.