Method for removing residual glue on surface of semiconductor and application of method

Through surface glue tearing, scratching, cleaning and annealing treatment, the problem of difficult removal of residual glue and impurities on the semiconductor surface is solved, the thorough cleaning of materials and the recycling of resources is achieved, the cleaning process is simplified, and it is suitable for small-scale research. .

CN118919397APending Publication Date: 2024-11-08GANNAN MEDICAL UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410946585.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the two-dimensional material mechanical cleavage technology, glue-like substances and impurities often remain on the semiconductor surface, making it difficult to reuse. The existing cleaning methods are complex and incomplete, resulting in waste of resources and impact on research results.

Method used

Using surface glue tearing, scratching, cleaning and annealing treatment, the surface of semiconductor materials is coated with glue layer, tearing off residual glue, scratching and removing impurities, using cleaning agent to remove residual glue and impurities, and annealing Thoroughly remove surface substances.

Benefits of technology

It achieves thorough cleaning of the surface of semiconductor materials, avoids waste of resources, simplifies the cleaning process, is suitable for small-scale research, and ensures the recyclability of semiconductor substrates and the accuracy of research results.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919397A_ABST
    Figure CN118919397A_ABST
Patent Text Reader

Abstract

The invention provides a method for removing residual glue on the surface of a semiconductor and application of the method. The method comprises the steps that S1, surface glue tearing treatment is carried out on the semiconductor material with the residual glue, specifically, the surface of the semiconductor material is covered with a glue layer, the glue layer at least covers the position of the residual glue, and the glue layer is torn off in the dry state of the glue layer; s2, performing scraping treatment on the semiconductor material treated in the S1; s3, putting the semiconductor material treated in the S2 into a first cleaning agent and enabling the first cleaning agent to submerge the surface, with the residual glue, of the semiconductor material, so as to clean the semiconductor material and obtain the semiconductor material with the basically clean surface; and S4, performing annealing treatment on the semiconductor material treated in the S3 to obtain the semiconductor material with a clean surface. According to the method provided by the invention, the residual glue and other impurities on the surface of the semiconductor material can be thoroughly removed, and the semiconductor material is not damaged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of semiconductor manufacturing, and in particular relates to a method for removing residual glue on the surface of a semiconductor and an application thereof. Background Art

[0002] Since the groundbreaking discovery and research of two-dimensional materials such as graphene, boron nitride, and transition metal disulfides (TMDs), the mechanical cleavage technology of two-dimensional materials has been promoted and applied by major laboratories in the past decade as a method that can quickly obtain two-dimensional materials with different numbers of layers through a non-growth method. In the research related to the interface between two-dimensional materials and semiconductors, it is necessary to transfer the two-dimensional materials after mechanical cleavage to the semiconductor surface through a transfer device. There are usually two ways to use mechanical cleavage technology for two-dimensional materials. The first way is to first use transparent tape or blue film tape to stick the two-dimensional material to be cleaved, fold it in half and tear it open several times, and then stick the cleaved two-dimensional material to the semiconductor surface for subsequent research. The second way is to first use tape to stick the pre-cleaved two-dimensional material to the surface of the Si-based material, and then use a PDMS film coated with a sticky adhesive such as PVA or PMMA on the surface to transfer the cleaved two-dimensional material to the target semiconductor surface for research through a transfer table.

[0003] However, no matter which method is used, after the two-dimensional material mechanical cleavage technology is applied to cleave the two-dimensional material and transfer the sample, a large amount of impurities and glue-like substances will inevitably be generated on the semiconductor surface. These glue-like substances and impurities will seriously affect the surface properties of the semiconductor. And considering that transfer failure may occur during the transfer, whether the sample transfer is successful or not, glue and impurities will remain on the semiconductor surface, making it difficult to reuse the semiconductor. Especially in the second method, the Si substrate material used is inevitably consumed and wasted. In small-scale research experiments, the number of semiconductor substrates that need to be cleaned is small, and it is usually not appropriate to use conventional industrial wafer cleaning technology, because the industrial cleaning method is more complicated and requires high precision for the cleaning instrument, which will lead to unnecessary cost increase. At present, water bath heating is usually used to remove the glue-like substances on the surface of these semiconductor substrates, but the water bath cleaning effect is poor, the removal effect of the glue-like substances is unsatisfactory, and other impurities cannot be effectively cleaned, resulting in the reuse of these semiconductor substrates. May affect the research results. Or, for semiconductor materials that cannot be thoroughly cleaned, they can usually only be directly discarded, resulting in serious waste. Summary of the invention

[0004] In order to solve all or part of the above technical problems, the present invention provides the following technical solutions:

[0005] One of the purposes of the present invention is to provide a method for removing residual adhesive on the surface of a semiconductor material, comprising:

[0006] S1: performing a surface glue peeling process on a semiconductor material with residual glue, including coating a glue layer on the surface of the semiconductor material, wherein the glue layer at least covers the position of the residual glue, and peeling off the glue layer when the glue layer is dry;

[0007] S2: Scratching the semiconductor material processed by S1;

[0008] S3: placing the semiconductor material processed by S2 in a first cleaning agent and making the first cleaning agent at least cover the surface of the semiconductor material with residual glue, thereby cleaning the semiconductor material to obtain a semiconductor material with a substantially clean surface;

[0009] S4: Annealing the semiconductor material processed in S3 to obtain a semiconductor material with a clean surface.

[0010] The method provided by the present invention can completely remove the residual glue and other impurities on the surface of the semiconductor material without causing damage to the semiconductor material; compared with the complex technology of conventional industrial wafer cleaning, the method provided by the present invention is simple and convenient, with low requirements for instruments and reagents, and is suitable for cleaning semiconductor materials with residual glue and impurities caused by small-scale research experiments and production, especially for laboratory preparation of two-dimensional material-semiconductor samples, which is used to completely remove the residual glue and impurities on the surface of the sample that failed to transfer or was consumed, so that the semiconductor substrate can be recycled, solving the serious waste problem caused by direct disposal in the prior art, or the problem that incomplete cleaning affects the research effect. Of course, this method is also applicable to semiconductor materials with residual glue on the surface obtained by other means.

[0011] In some embodiments, the glue forming the glue layer includes PVA (polyvinyl alcohol) and / or PMMA (polymethyl methacrylate), but is not limited thereto. It can be imagined that the glue layer formed by other glue solutions can also achieve the purpose of removing part of the residual glue during the glue tearing process. Since the glue used for the cleavage transfer of two-dimensional materials is generally PVA and PMMA, from the perspective of not introducing other impurity components, PVA glue or PMMA glue is preferably used. In addition, through effect comparison, it is found that compared with PMMA glue, the effect of surface film tearing using PVA glue is better, and most of the original residual glue and impurities can be torn off together with the PVA film, and the covered PVA film can be completely torn off and is not easy to remain on the semiconductor surface. Therefore, in some preferred embodiments, the glue includes PVA, especially a glue layer formed by a saturated PVA solution.

[0012] In some embodiments, the glue also includes 5-7% by volume of ethanol, less than 9% by volume of glycerol, and 1.8-2.45wt% of gelatin powder. Adding ethanol, glycerol, and gelatin powder to the glue can make the formed glue layer more flexible, and make the glue layer not too firmly adhere to the surface of the semiconductor material, and it is not easy to cause the film chain breakage problem when the film is torn off; and the effect is better when the three are used in combination. If one or two of them are used alone, the improvement in flexibility is not significant. The amount of glycerol added is more suitable below 9% by volume, for example 1-9%.

[0013] In some embodiments, the surface glue peeling process specifically includes: coating the entire surface of the semiconductor material with residual glue with glue to form a glue layer covering the entire surface, then heating and drying the glue layer to form a dry glue layer, and then tearing off the glue layer. Covering the entire surface of the semiconductor with a glue layer is not easy to introduce bubbles and excessive gaps, and the glue peeling effect is better; rapid drying can make the glue and the semiconductor material fit more evenly and firmly. Heating can accelerate drying. Compared with natural drying at room temperature, heating promotes the glue layer and the surface residual glue to be more tightly combined due to the action of van der Waals force, making the residual glue easier to remove during the glue peeling process.

[0014] In some embodiments, when the solvent of the glue is water, the temperature of the heating and drying is 75-100° C., and the drying time is 5-10 minutes.

[0015] In the embodiment where the glue contains ethanol, the temperature of the heating and drying is 40-55° C., and the drying time is, for example, 8 to 10 minutes. In this case, the drying temperature should not be too high, otherwise the ethanol will evaporate quickly and affect the flexibility of the glue layer.

[0016] In some embodiments, the scraping treatment specifically includes: scraping the surface of the semiconductor material once or multiple times with a flat scraper, the portion of the flat scraper in contact with the surface of the semiconductor material is provided with a wiping material, and the wiping material is soaked with a second cleaning agent.

[0017] In some embodiments, the second cleaning agent includes acetone.

[0018] In some embodiments, the wiping material is dust-free wiping paper.

[0019] In some embodiments, the wiping material is replaced during multiple scraping processes.

[0020] In some embodiments, the method further comprises: after the scraping is completed, ultrasonically cleaning the scraped semiconductor material, and then performing S3.

[0021] In some embodiments, the first cleaning agent includes water and / or acetone.

[0022] In some embodiments, the semiconductor material is placed in a first cleaning agent and the temperature is adjusted to 50-60°C.

[0023] In some embodiments, S3 specifically includes:

[0024] S3a: placing the semiconductor material in a first cleaning agent containing water, and then heating to 55-75° C. and maintaining for 45-65 minutes to remove at least part of the PVA residual adhesive;

[0025] S3b: placing the semiconductor material in a first cleaning agent containing acetone for one or more heating cleanings, each heating cleaning temperature being 45 to 75° C. and maintained for 30 to 40 minutes, so as to remove at least part of the PMMA residual glue;

[0026] Among them, when the residual glue contains PVA but not PMMA, only S3a is executed; when the residual glue contains PMMA but not PVA, only S3b is executed; when the residual glue contains both PVA and PMMA, S3a and S3b are executed, and the order of S3a and S3b is not restricted.

[0027] In some embodiments, in the case where the residual adhesive contains PMMA, before heating, the semiconductor material is placed in room temperature acetone and allowed to stand for one or more times, each time for 30N40min, and the acetone is replaced each time. Using room temperature acetone first and then acetone heating cleaning can remove the PMMA remaining on the surface to the maximum extent.

[0028] In some embodiments, the annealing treatment temperature is 450-500° C., the heating rate is 5-15° C. / min, and the holding time is 1.5-2 h.

[0029] In some embodiments, the atmosphere used for the annealing treatment includes an inert atmosphere. Preferably, the atmosphere used for annealing is a mixed atmosphere of hydrogen and an inert gas. For example, pure argon gas can be introduced for 15-20 minutes to drive out the gas, and then a mixed atmosphere of hydrogen and argon can be introduced, and heating and annealing can be completed in the mixed gas phenol. The mixed atmosphere of hydrogen and inert gas can effectively remove residual glue on the surface at a high temperature of more than 400°C, and the hydrogen therein can preferentially saturate the dangling bonds on the surface of semiconductor materials (such as silicon and germanium materials), and reduce surface recombination centers.

[0030] In some embodiments, the volume ratio of hydrogen to argon in the mixed atmosphere is 35:65 to 60:40.

[0031] In some embodiments, the inert gas is argon and / or helium.

[0032] In some embodiments, the rate of introducing the atmosphere during the annealing process is 1500-2500 sccm.

[0033] In some embodiments, the semiconductor material includes a first generation semiconductor material, a second generation semiconductor material, or a third generation semiconductor material, such as a Si-based material, a gallium arsenide material, or a gallium nitride material.

[0034] The second object of the present invention is to provide an application of the method described in any of the above technical solutions in removing residual glue on the surface of a semiconductor substrate for mechanical cleavage and transfer of two-dimensional materials.

[0035] Compared with the prior art, the present invention has at least the following beneficial effects:

[0036] (1) The method provided by the present invention can completely remove the residual glue and other impurities on the surface of the semiconductor material without causing damage to the semiconductor material. Compared with the complex technology of conventional industrial cleaning of semiconductors such as wafers, the method provided by the present invention is simple and convenient, with low requirements for instruments, equipment and reagents. It is suitable for cleaning semiconductor materials with residual glue and impurities caused by small-scale research experiments and production, especially for laboratory preparation of two-dimensional material-semiconductor samples, it is used to completely remove the residual glue and impurities on the surface of the sample where the two-dimensional material transfer failed or was consumed, so that the semiconductor substrate can be recycled, solving the serious waste problem caused by direct disposal in the prior art, or the problem that incomplete cleaning affects the subsequent effect;

[0037] (2) Furthermore, the present invention adds ethanol, glycerin and gelatin powder to the glue to form a glue layer with moderate flexibility and achieve a good film tearing effect;

[0038] (3) Furthermore, the present invention has found that in the drying process of the glue layer, heating and drying it can improve the effect of removing residual glue compared to air-drying at room temperature. This may be because the heating process can promote the Van der Waals force between the glue layer and the surface residual glue to be more tightly bonded, making the residual glue easier to remove during the glue peeling process. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0040] Figure 1 is a flow chart of a method for removing residual adhesive from a semiconductor surface in one embodiment of the present invention;

[0041] Figure 2 The residual glue and impurities on the surface of the semiconductor material without any cleaning after the cleavage and transfer of the two-dimensional material in Example 1 of the present invention;

[0042] Figure 3 is a microscope image of the semiconductor surface after the surface adhesive peeling treatment in Example 1 of the present invention;

[0043] Figure 4 is a microscope image of the semiconductor surface after annealing in Example 1 of the present invention;

[0044] Figure 5 This is a microscope image of the semiconductor surface after cleaning by the method of Comparative Example 1. DETAILED DESCRIPTION

[0045] The technical solution of the present invention is described in detail below in conjunction with specific embodiments so that those skilled in the art can better understand and implement the technical solution of the present invention. The specific functional details disclosed herein should not be interpreted as limiting, but only as the basis for the claims and as a representative basis for teaching those skilled in the art to adopt the present invention in different ways in any appropriate detailed embodiment.

[0046] Unless otherwise specified, the raw materials and reagents used in the present invention are all commercially available.

[0047] Example 1

[0048] This embodiment provides a method for removing residual glue on the surface of a semiconductor. Figure 2 The semiconductor surface is not cleaned, the semiconductor is a Si-based semiconductor, the source of the residual glue is the glue remaining on the semiconductor substrate after the cleavage and transfer of the two-dimensional material, and there are other impurities on the surface. The process of the method provided in this embodiment is as follows Figure 1 As shown, the details are as follows:

[0049] (1) Surface peeling process:

[0050] ①Prepare saturated PVA solution:

[0051] Use a clean beaker to hold 100 ml of ultrapure water, then use a small spoon to hold solid polyvinyl alcohol (the degree of alcoholysis of the polyvinyl alcohol used is 98.0-99.0 mol%, and the viscosity is 54.0-66.0 mPa.s), slowly disperse and add it into the beaker containing ultrapure water, stir slowly with a glass rod while adding, and prevent the liquid from splashing; when there is about 1-2 mm thick polyvinyl alcohol precipitation at the bottom of the beaker, stop adding polyvinyl alcohol;

[0052] The beaker containing the polyvinyl alcohol solution is left to stand at room temperature for 10-15 minutes, and is continuously stirred slowly with a stirring rod to allow the solid particles to swell in the deionized water, ensuring that the next step of heating and dissolution can be fully completed;

[0053] Put a capsule-shaped magnetic stirrer in a beaker and place it on a magnetic stirrer. Heat to 70°C and maintain stirring for 6 hours. Observe every hour during the process. If there are particles that are not completely dissolved, add a small amount of deionized water several times to allow the polyvinyl alcohol particles to fully dissolve. When stirring with a magnetic stirrer, seal the beaker mouth with plastic wrap to prevent the solution from splashing and a small amount of water from evaporating due to stirring. After heating and dissolving, a saturated PVA solution is obtained.

[0054] ② Spin coating PVA

[0055] Place the semiconductor material on the rotating table of the glue spreader, with the side with residual glue and impurities facing up, and turn on the vacuum pump of the glue spreader to prevent the material from flying out during rotation;

[0056] Use a pipette to absorb the prepared saturated PVA solution, and evenly spin-coat a layer of glue on the surface of the semiconductor material, and spin-coat the entire surface evenly with glue;

[0057] Turn on the glue spreader and spin the glue twice. The spin coating parameters are set as follows: speed: 200 rpm, time: 15 s, acceleration: 100 rpm / s; speed: 1500 rpm, time: 25 s, acceleration: 100 rpm / s.

[0058] After spin coating, place in a 100°C oven for 7 min, then place in an electronic moisture-proof cabinet to dry naturally for 12 h;

[0059] ③ Surface peeling

[0060] After the surface of the semiconductor material is naturally dried, place it on a clean glass slide. At this time, there is a layer of transparent adhesive film completely attached to the surface of the semiconductor material. Use clean tweezers to gently pinch a corner of the film and slowly tear it off. At this time, most of the residual glue and impurities on the surface of the semiconductor will be torn off together with the film. This step is not only simple and convenient to operate, but also can remove most of the residual glue and impurities on the surface without damaging the surface of the semiconductor material. Figure 3 The semiconductor surface has been treated by the surface peeling process, and the impurities and residual glue are significantly reduced;

[0061] (2) Scraping process

[0062] Use flat-tipped tweezers, wrap the top of the tweezers with dust-free lens cleaning paper, dip a small amount of acetone into the dust-free lens cleaning paper, and wipe the surface of the material after the glue peeling process in a fume hood; change the dust-free lens cleaning paper three times in the middle, and wipe repeatedly until there is no impurity on the surface;

[0063] Place the scraped semiconductor material with the surface facing up in a clean beaker, add an appropriate amount of deionized water, and place it in an ultrasonic cleaning machine for cleaning. The parameters are set to power P: 50W, Tm: 30℃, Ti: 20min;

[0064] The scraping step can remove impurities on the surface of the semiconductor material that have not been removed by the adhesive stripping process, leaving only a small amount of adhesive residue on the surface;

[0065] (3) Removal of PVA

[0066] Take out the semiconductor material cleaned by the ultrasonic cleaner, place it in a new clean beaker, add an appropriate amount of ultrapure water, seal it with plastic wrap and place it in a 60°C constant temperature water bath for 1 hour to basically remove the PVA glue remaining on the surface of the semiconductor material;

[0067] (4) Removal of PMMA

[0068] The semiconductor material treated in step (3) is taken out and placed in a 50°C oven for drying for 10 minutes. The semiconductor material is taken out and placed in a newly prepared clean beaker. An appropriate amount of room temperature acetone solution is added to the beaker in a fume hood so that the acetone solution just covers the surface of the material. The beaker is then sealed with plastic wrap and allowed to stand for ten minutes. Then, a new acetone solution is replaced and the step is repeated three times. This step can remove the PMMA remaining on the surface.

[0069] Take out the semiconductor material treated with room temperature acetone, replace it with a new clean beaker, add an appropriate amount of acetone solution to the beaker in a fume hood, seal it with plastic wrap, put it in a water bath and heat it at 50°C for 30 minutes, then replace it with new acetone solution, and repeat the steps three times to deeply remove the PMMA remaining on the surface;

[0070] After completing the above steps, take out the semiconductor material and put it into a clean beaker, add an appropriate amount of deionized water, and put it into an ultrasonic cleaner for cleaning. The parameters are set to power P: 50W, Tm: 30℃, Ti: 10min, and change the deionized water twice to remove the residual acetone on the surface of the material. Then take out the material and put it into an electronic moisture-proof cabinet to dry naturally for 24 hours.

[0071] (5) Annealing process

[0072] Put the semiconductor material into a clean ceramic crucible and place it in a tube furnace. Evacuate it three times and use argon to expel the gas for no less than 10 minutes. Then, introduce hydrogen and argon at a volume ratio of 45:55 and a ventilation rate of 2000sccm. Heat up and anneal in a mixed atmosphere of hydrogen and argon at a heating rate of 5°C / min. The final temperature is set to 500°C and kept warm for two hours for annealing to completely remove PVA, PMMA and other adhesives remaining on the surface of the semiconductor material.

[0073] Figure 4 This is a microscope picture of the semiconductor surface after the above five-step treatment procedure. The glue and impurities on the semiconductor surface are removed more thoroughly, no impurities and residual glue are found, and the semiconductor surface is not damaged, indicating that this treatment process can be used for laboratory processing of semiconductor materials after two-dimensional material transfer, so that they can be reused.

[0074] Example 2

[0075] The semiconductor material targeted by Example 2 is a case where PVA glue is used to transfer a two-dimensional material to leave PVA residual glue on the semiconductor surface. The semiconductor material is a Si-based semiconductor. The only difference between Example 2 and Example 1 is that there is no need to perform step (4) to remove PMMA. The rest is implemented in the same way as Example 1, and the cleaning effect is equivalent to that of Example 1.

[0076] In addition, the present invention also uses the above method to clean the surface of semiconductor substrates made of gallium arsenide and gallium nitride. It is found that the method provided by the present invention can achieve good cleaning effects for semiconductor materials of different materials. There is basically no residual glue and impurities on the surface, and it will not cause damage to the surface of the semiconductor substrate.

[0077] Example 3

[0078] The surface adhesive peeling process of Example 3 is as follows:

[0079] ①Prepare PVA solution:

[0080] Use a clean beaker to hold 100 ml of ultrapure water, then use a small spoon to hold solid polyvinyl alcohol (the degree of alcoholysis of the polyvinyl alcohol used is 98.0-99.0 mol%, and the viscosity is 54.0-66.0 mPa.s), slowly disperse and add it into the beaker containing ultrapure water, stir slowly with a glass rod while adding, and prevent the liquid from splashing; when there is a polyvinyl alcohol precipitation of about 1-2 mm thick at the bottom of the beaker, stop adding polyvinyl alcohol;

[0081] The beaker containing the polyvinyl alcohol solution is left to stand at room temperature for 10-15 minutes, and is continuously stirred slowly with a stirring rod to allow the solid particles to swell in the deionized water, ensuring that the next step of heating and dissolution can be fully completed;

[0082] Put a capsule-shaped magnetic stirrer in a beaker and place it on a magnetic stirrer. Heat to 70°C and maintain stirring for 6 hours. Observe every hour during the process. If there are particles that are not completely dissolved, add a small amount of deionized water several times to allow the polyvinyl alcohol particles to fully dissolve. When stirring with a magnetic stirrer, seal the beaker mouth with plastic wrap to prevent the solution from splashing and a small amount of water from evaporating due to stirring. After heating and dissolving, a saturated PVA solution is obtained.

[0083] Dissolve gelatin powder in an appropriate amount of ultrapure water and slowly heat in a 60°C water bath until the gelatin powder is completely dissolved to obtain a gelatin powder solution with a concentration of 0.02 g / ml;

[0084] 100% concentration of anhydrous ethanol, glycerin and the above-mentioned gelatin powder solution are added to the above-mentioned saturated PVA solution in sequence to obtain glue for forming a glue layer; wherein the added volume of anhydrous ethanol accounts for 6% of the total volume of the glue, the volume of glycerin is 9%, and the added amount of gelatin powder is 2wt%.

[0085] ② Spin coating PVA

[0086] Place the semiconductor material on the rotating table of the glue spreader, with the side with residual glue and impurities facing up, and turn on the vacuum pump of the glue spreader to prevent the material from flying out during rotation;

[0087] Use a pipette to absorb the prepared glue, and evenly spin-coat a layer of glue on the surface of the semiconductor material, until the entire surface is evenly coated with glue;

[0088] Turn on the glue spreader and spin the glue twice. The spin coating parameters are set as follows: speed: 200 rpm, time: 15 s, acceleration: 100 rpm / s; speed: 1500 rpm, time: 25 s, acceleration: 100 rpm / s.

[0089] After spin coating, place the plate in a 50°C oven for 10 min, then place it in an electronic moisture-proof cabinet to dry naturally for 12 h;

[0090] ③ Surface peeling

[0091] After the surface of the semiconductor material is naturally dried, it is placed on a clean glass slide. At this time, there is a layer of transparent adhesive film completely attached to the surface of the semiconductor material. Use clean tweezers to gently clamp a corner of the film and slowly tear it off. At this time, most of the residual glue and impurities on the surface of the semiconductor will be torn off together with the film. Comparing Examples 1 and 3, it is found that the glue layer formed by adding ethanol, glycerin and gelatin powder is more uniform and flexible, has better adhesion to the semiconductor material, and is not prone to breakage when torn off.

[0092] (2) Scraping process

[0093] Use flat-tipped tweezers, wrap the top of the tweezers with dust-free lens cleaning paper, dip a small amount of acetone into the dust-free lens cleaning paper, and wipe the surface of the material after the glue peeling process in a fume hood; change the dust-free lens cleaning paper three times in the middle, and wipe repeatedly until there is no impurity on the surface;

[0094] Place the scraped semiconductor material with the surface facing up in a clean beaker, add an appropriate amount of deionized water, and place it in an ultrasonic cleaning machine for cleaning. The parameters are set to power P: 50W, Tm: 30℃, Ti: 20min;

[0095] The scraping step can remove impurities on the surface of the semiconductor material that have not been removed by the adhesive stripping process, leaving only a small amount of adhesive residue on the surface;

[0096] (3) Removal of PVA

[0097] Take out the semiconductor material cleaned by the ultrasonic cleaner, place it in a new clean beaker, add an appropriate amount of ultrapure water, seal it with plastic wrap and place it in a 55°C constant temperature water bath for 45 minutes to basically remove the PVA glue remaining on the surface of the semiconductor material;

[0098] (4) Removal of PMMA

[0099] The semiconductor material treated in step (3) is taken out and placed in a 50°C oven for drying for 10 minutes. The semiconductor material is taken out and placed in a newly prepared clean beaker. An appropriate amount of room temperature acetone solution is added to the beaker in a fume hood so that the acetone solution just covers the surface of the material. The beaker is then sealed with plastic wrap and allowed to stand for ten minutes. Then, a new acetone solution is replaced and the step is repeated three times. This step can remove the PMMA remaining on the surface.

[0100] Take out the semiconductor material treated with room temperature acetone, replace it with a new clean beaker, add an appropriate amount of acetone solution to the beaker in a fume hood, seal it with plastic wrap, put it in a water bath and heat it at 45°C for 40 minutes, then replace it with new acetone solution, and repeat the steps three times to deeply remove the PMMA remaining on the surface;

[0101] After completing the above steps, take out the semiconductor material and put it into a clean beaker, add an appropriate amount of deionized water, and put it into an ultrasonic cleaner for cleaning. The parameters are set to power P: 50W, Tm: 30℃, Ti: 10min, and change the deionized water twice to remove the residual acetone on the surface of the material. Then take out the material and put it into an electronic moisture-proof cabinet to dry naturally for 24 hours.

[0102] (5) Annealing process

[0103] The semiconductor material is placed in a clean ceramic crucible and placed in a tube furnace. The vacuum is drawn three times and the crucible is degassed with argon for no less than 10 minutes. Then, hydrogen and argon are introduced at a volume ratio of 45:55 and a ventilation rate of 2000sccm. The temperature is raised and annealed in a mixed atmosphere of hydrogen and argon at a heating rate of 15°C / min. The final temperature is set to 450°C and kept warm for two hours for annealing to completely remove PVA, PMMA and other adhesives remaining on the surface of the semiconductor material.

[0104] Example 4

[0105] The only difference between Example 4 and Example 3 is that 5% by volume of anhydrous ethanol, 6% by volume of glycerol and 1.8wt% of gelatin powder are added to the prepared saturated PVA solution; and the atmosphere used in the annealing process is hydrogen and argon in a volume ratio of 35:65, and the effect obtained is equivalent to that of Example 3.

[0106] Example 5

[0107] The only difference between Example 5 and Example 3 is that 7% by volume of anhydrous ethanol, 1% by volume of glycerol and 2.45wt% of gelatin powder are added to the prepared PVA solution, and the atmosphere used in the annealing process is hydrogen and argon in a volume ratio of 60:40. The effect obtained is equivalent to that of Example 3.

[0108] Example 6

[0109] The only difference between Example 6 and Example 1 is that during the annealing process, the atmosphere used is pure argon atmosphere, and the rest is implemented in the same way as Example 1. Compared with Example 6, the annealing in Example 1 using a mixed atmosphere of hydrogen and argon can more effectively remove the residual glue on the surface, and hydrogen can effectively saturate the dangling bonds on the surface of semiconductors (such as silicon, germanium, etc.) and reduce surface recombination centers; of course, in some embodiments with lower requirements, only using pure argon atmosphere annealing can also meet the cleaning effect, which can be specifically selected based on the subsequent application requirements of the semiconductor material.

[0110] Comparative Example 1

[0111] The difference between Comparative Example 1 and Example 1 is that the surface peeling and scraping process is not performed, and the remaining PVA, PMMA removal and annealing processes are implemented in the same manner as in the above example. Figure 5 This is a diagram of residual glue and impurities on the surface of the treated semiconductor. It can be seen that the removal effect of residual glue and impurities is poor.

[0112] Comparative Example 2

[0113] The difference between Comparative Example 2 and Example 1 is that the surface adhesive peeling process is not performed, and the remaining scraping processes, removal of PVA, PMMA and annealing processes are implemented in the same manner as the above examples. Compared with Example 1, the removal effect is poor.

[0114] Comparative Example 3

[0115] The difference between Comparative Example 3 and the above-mentioned embodiment is that no scraping process is performed, and the remaining surface glue peeling, PVA, PMMA removal and annealing processes are implemented in the same manner as the above-mentioned embodiment, and the removal effect is poor compared with that of Embodiment 1.

[0116] In summary, the present invention provides a semiconductor material surface cleaning process, which can be used at least in the laboratory to thoroughly remove the residual glue and impurities on the surface of the sample that failed to transfer or was consumed after preparing the two-dimensional material-semiconductor sample. This method is not limited to removing the glue and impurities remaining on the semiconductor after the cleavage and transfer of the two-dimensional material, but can also be used to remove the residual glue and impurities on the semiconductor surface caused by other means. This method circumvents the complex technology of conventional industrial wafer cleaning and the requirements for precision cleaning instruments, and is more suitable for conventional laboratory requirements. The cleaning process is simple and convenient, and the requirements for the equipment required for cleaning are relatively low.

[0117] The various aspects, embodiments, features and examples of the present invention should be considered as illustrative in all aspects and are not intended to limit the present invention, the scope of the present invention is defined only by the claims. Other embodiments, modifications and uses will be apparent to those skilled in the art without departing from the spirit and scope of the claimed invention.

[0118] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.

[0119] Although the present invention has been described with reference to illustrative embodiments, it will be appreciated by those skilled in the art that various other changes, omissions and / or additions may be made without departing from the spirit and scope of the present invention and that the elements of the embodiments may be replaced by substantial equivalents. In addition, many modifications may be made without departing from the scope of the present invention to adapt specific circumstances or materials to the teachings of the present invention. Therefore, it is not intended herein to limit the present invention to the disclosed specific embodiments for performing the present invention, but it is intended that the present invention will include all embodiments within the scope of the appended claims. In addition, unless specifically stated, any use of the terms first, second, etc. does not indicate any order or importance, but rather uses the terms first, second, etc. to distinguish one element from another.

Claims

1. A method for removing residual glue from the surface of a semiconductor material, characterized in that: include: S1: performing a surface glue peeling process on a semiconductor material with residual glue, including coating a glue layer on the surface of the semiconductor material, wherein the glue layer at least covers the position of the residual glue, and peeling off the glue layer when the glue layer is dry; S2: Scratching the semiconductor material processed by S1; S3: placing the semiconductor material processed by S2 in a first cleaning agent and allowing the first cleaning agent to cover the surface of the semiconductor material with residual glue, thereby cleaning the semiconductor material to obtain a semiconductor material with a substantially clean surface; S4: Annealing the semiconductor material processed in S3 to obtain a semiconductor material with a clean surface.

2. The method according to claim 1, characterized in that: The glue forming the glue layer includes PVA and / or PMMA; Preferably, the glue further comprises 5-7% by volume of ethanol, less than 9% by volume of glycerin and 1.8-2.45 wt % of gelatin powder; preferably, the glue comprises PVA.

3. The method according to claim 2, characterized in that The surface glue peeling process specifically includes: coating the entire surface of the semiconductor material with residual glue with glue to form a glue layer covering the entire surface, then heating and drying the glue layer to form a dry glue layer, and then peeling off the glue layer; Preferably, the temperature of the heating and drying is 40-55° C., and the time is 8-10 minutes.

4. The method according to claim 1, characterized in that: The scraping treatment specifically includes: scraping the surface of the semiconductor material once or multiple times with a flat scraper, the portion of the flat scraper in contact with the surface of the semiconductor material is provided with a wiping material, and the wiping material is soaked with a second cleaning agent; Preferably, the second cleaning agent comprises acetone; Preferably, the wiping material is dust-free wiping paper; Preferably, the wiping material is replaced during multiple scraping processes; Preferably, after the scraping is completed, the scraped semiconductor material is ultrasonically cleaned, and then the step S3 is performed.

5. The method according to claim 1, characterized in that: The first cleaning agent includes water and / or acetone; And / or, placing the semiconductor material in a first cleaning agent and adjusting the temperature to 50-60°C.

6. The method according to claim 5, characterized in that: The S3 specifically includes: S3a: placing the semiconductor material in a first cleaning agent containing water, and then heating to 55-75° C. and maintaining for 45-65 minutes to remove at least part of the PVA residual adhesive; S3b: placing the semiconductor material in a first cleaning agent containing acetone for one or more heating cleanings, each heating cleaning temperature being 45 to 75° C. and maintained for 30 to 40 minutes, so as to remove at least part of the PMMA residual glue; Among them, when the residual glue contains PVA but not PMMA, only S3a is executed; when the residual glue contains PMMA but not PVA, only S3b is executed; when the residual glue contains both PVA and PMMA, S3a and S3b are executed, and the order of S3a and S3b is not restricted.

7. The method according to claim 6, characterized in that: In the case where the residual glue contains PMMA, before heating, place the semiconductor material in acetone at room temperature and let it stand once or more, each time for 30-40 minutes, and replace the acetone each time.

8. The method according to claim 1, characterized in that: The annealing treatment temperature is 450-500°C, the heating rate is 5-15°C / min, and the holding time is 1.5-2h; And / or, the atmosphere used for the annealing treatment is a mixed atmosphere of hydrogen and inert gas, preferably, the volume ratio of hydrogen to inert gas is 35:65-60:40, preferably, the introduction rate of the atmosphere is 1500-2500sccm, preferably, the inert gas is argon and / or helium.

9. The method according to claims 1 to 8, characterized in that: The semiconductor material is a Si-based material, a gallium arsenide material or a gallium nitride material.

10. Use of the method according to claims 1 to 9 in removing residual adhesive on the surface of a semiconductor substrate for mechanical cleavage transfer of two-dimensional materials.

Citation Information

Cited By

  • Method for removing residual adhesive on surface of two-dimensional material after mechanical cleavage of adhesive tape

    CN119819651A