Separator for electrochemical device comprising organic / inorganic composite porous coating layer, and electrochemical device comprising same
By using organic/inorganic composite porous coating on the separator of the electrochemical device, including fluoropolymer and acrylic polymer particles, the problems of reducing thickness and deformation of the pore structure under high pressure are solved, and high viscosity is achieved Combination and stability improve the thermal stability and dielectric characteristics of the battery.
Patent Information
- Application Number
- CN202380027554.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-26
- Filing Date
- 2023-03-07
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-03-07
AI Technical Summary
The separators in the existing electrochemical devices are prone to decrease in thickness of the porous polymer substrate and deformation of the pore structure under high pressure, resulting in deterioration of dielectric properties and insufficient adhesion under dry and wet conditions, which poses a risk of separation.
Using organic/inorganic composite porous coatings, mixed polymer particles containing fluorine-based polymers and acrylic polymers, as well as acrylic polymer particles, the particle size and proportions are optimized to form compression resistance and high adhesion .
The bonding force of the separator under wet and dry conditions is improved, the risk of dielectric deterioration and separation is prevented, and the shape stability and thermal stability of the electrode assembly are enhanced.
Smart Images

Figure CN118922994A_ABST
Abstract
Description
Technical Field
[0001] This application claims priority to Korean Patent Application No. 10-2022-0064640, filed on May 26, 2022, the entire contents of which are incorporated herein by reference for all purposes. The present disclosure relates to an electrochemical device separator having improved compression resistance, adhesion in a dry state (dry adhesion), and adhesion in an electrolyte-impregnated state (wet adhesion), and to an electrochemical device including the same. Background Art
[0002] Electrochemical devices such as lithium secondary batteries are generally composed mainly of a cathode, a separator, an anode, and an electrolyte solution. Electrochemical devices are high-density energy storage devices that can be charged and discharged through reversible conversion between chemical energy and electrical energy, and are widely used in small electronic devices such as mobile phones and laptops. Recently, the application of electrochemical devices has rapidly expanded to hybrid electric vehicles (HEVs), plug-in EVs, electric bicycles, and energy storage systems (ESSs) to address environmental issues, high oil prices, energy efficiency, and energy storage.
[0003] Ensuring the safety of such electrochemical devices is a major concern during their manufacture and use. Specifically, separators made from porous polymer substrates, commonly used in electrochemical devices, exhibit extreme thermal shrinkage at high temperatures, due to their material properties and manufacturing process characteristics, leading to internal short circuits. Recently, to ensure the safety of lithium secondary batteries, separators have been developed that utilize a porous polymer substrate coated with a mixture of inorganic particles and a binder polymer to form an organic / inorganic composite porous coating.
[0004] Typically, electrode assemblies are manufactured by a lamination process in which the separator and the electrode are bonded by heat and pressure, and the higher the heat and pressure applied in the process, the higher the bonding force between the electrode and the separator. Recently, due to the increase in processing speed for the purpose of improving productivity, the time for applying heat to the separator has been shortened. However, due to the high pressure, the organic / inorganic composite porous coating squeezes the porous polymer substrate, thereby reducing the thickness and causing deformation of the pore structure. When the inorganic particles locally aggregate or form protrusions, the porous polymer substrate may be destroyed, and therefore there is a problem of possible dielectric degradation of the separator.
[0005] On the other hand, when forming an electrode assembly by laminating an electrode and a separator having an organic / inorganic composite porous coating, there is a high risk that the electrode and separator may separate due to insufficient adhesion, and in this case, the inorganic particles released during the separation process may act as local defects in the device. Therefore, a separator in which an acrylic polymer binder is applied to the organic / inorganic composite porous coating to improve the adhesion between the electrode and the separator has been proposed. However, when using an acrylic polymer binder, dry adhesion is improved, but there is a problem that after application to the battery, wet adhesion is reduced due to problems such as swelling or dissolution of the acrylic polymer binder by the electrolyte. Summary of the Invention
[0006] Technical issues
[0007] One object of the present disclosure is to provide a separator for an electrochemical device, wherein the phenomenon of reduced dielectric properties of the separator, such as reduction in thickness of a porous polymer substrate or deformation of the pore structure due to high voltage applied when laminating a separator having an organic / inorganic composite porous coating on at least one side of the porous polymer substrate and an electrode, is improved, and at the same time, the bonding force with the electrode can be improved under both dry and wet conditions.
[0008] Furthermore, another object of the present disclosure is to provide an electrochemical device including a separator having the above-mentioned characteristics.
[0009] Other purposes and advantages of the present disclosure will be understood from the following description.On the other hand, it will be easily understood that the purposes and advantages of the present disclosure can be achieved by the means or methods described in the claims and their combinations.
[0010] Technical Solution
[0011] A first aspect of the present disclosure relates to a separator for an electrochemical device,
[0012] The separator includes a porous polymer substrate and an organic / inorganic composite porous coating layer formed on at least one side of the polymer substrate.
[0013] wherein the organic / inorganic composite porous coating comprises a particulate binder polymer and first inorganic particles,
[0014] The particulate binder polymer comprises hybrid polymer particles of a fluorine-based polymer and an acrylic polymer, and acrylic polymer particles,
[0015] The particle size D50(a) of the acrylic polymer particles is in the range of 1 μm to 7 μm,
[0016] The particle size D50(b) of the first inorganic particles is in the range of 200 nm to 800 nm, a / b is 2 to 15,
[0017] And the particle size D50 of the hybrid polymer particles is smaller than the particle size D50 of the acrylic polymer particles.
[0018] The second aspect of the present disclosure is that in the first aspect, the particle size D50(a) of the acrylic polymer particles is in the range of 2μm to 6μm, and the particle size D50(b) of the first inorganic particles is in the range of 300nm to 700nm, and a / b is 5 to 12.
[0019] A third aspect of the present disclosure is that in the first aspect or the second aspect, the particle size D50 of the acrylic polymer particles is 4 to 20 times larger than the particle size D50 of the hybrid polymer particles.
[0020] A fourth aspect of the present disclosure is that, in any one of the first to third aspects, the average particle diameter (D50) of the hybrid polymer particles is within a range of 100 nm to 500 nm.
[0021] A fifth aspect of the present disclosure is that, in any one of the first to fourth aspects, a mixing weight ratio of the hybrid polymer particles and the acrylic polymer particles is 8:2 to 2:8.
[0022] A sixth aspect of the present disclosure is that, in any one of the first to fifth aspects, Tg of the acrylic polymer contained in the hybrid polymer particles is 10° C. or more lower than Tg of the acrylic polymer contained in the acrylic polymer particles.
[0023] A seventh aspect of the present disclosure is that in the sixth aspect, the Tg of the acrylic polymer contained in the hybrid polymer particles is 10°C to 30°C, and the Tg of the acrylic polymer contained in the acrylic polymer particles is 30°C to 50°C.
[0024] An eighth aspect of the present disclosure is that in any one of the first to seventh aspects, the fluorine-based polymer is a homopolymer of vinylidene fluoride, a copolymer of vinylidene fluoride and other polymerizable monomers, or a mixture of two or more thereof.
[0025] A ninth aspect of the present disclosure is that in the eighth aspect, the monomer is at least one selected from the group consisting of tetrafluoroethylene, hexafluoropropylene, trifluoroethylene, chlorofluoroethylene, 1,2-difluoroethylene, perfluoro(methyl vinyl) ether, perfluoro(ethyl vinyl) ether, perfluoro(propyl vinyl) ether, perfluoro(1,3-dioxole), perfluoro(2,2-dimethyl-1,3-dioxole), trichloroethylene, and vinyl fluoride.
[0026] A tenth aspect of the present disclosure is that in the eighth aspect, the fluorine-based polymer is a copolymer of vinylidene fluoride and hexafluoropropylene.
[0027] An eleventh aspect of the present disclosure is that in the eighth aspect, the content of the monomer is 1 to 20 weight % of the copolymer.
[0028] The twelfth aspect of the present disclosure is that in any one of the first to eleventh aspects, the acrylic polymer constituting the hybrid polymer particles and the acrylic polymer constituting the acrylic polymer particles each independently contain a (meth)acrylate repeating unit having an alkyl group having 1 to 18 carbon atoms.
[0029] A thirteenth aspect of the present disclosure is that in any one of the first to twelfth aspects, the organic / inorganic composite porous coating further includes a non-particulate acrylic polymer.
[0030] A fourteenth aspect of the present disclosure is that in the thirteenth aspect, the non-granular acrylic polymer has a Tg of 0° C. or lower.
[0031] A fifteenth aspect of the present disclosure is that in any one of the first to fourteenth aspects, the organic / inorganic composite porous coating layer includes second inorganic particles different from the first inorganic particles, and the particle size D50 of the second inorganic particles is smaller than the particle size D50 of the first inorganic particles.
[0032] A sixteenth aspect of the present disclosure is that in the fifteenth aspect, a particle diameter (D50) of the second inorganic particles is within a range of 100 nm to 500 nm.
[0033] A seventeenth aspect of the present disclosure is that in the fifteenth aspect, the first inorganic particles are alumina, and the second inorganic particles are boehmite.
[0034] An eighteenth aspect of the present disclosure is that in any one of the first to seventeenth aspects, the organic / inorganic composite porous coating layer comprises a particulate binder polymer in an amount of 1 wt % to 30 wt % based on the total weight of the organic / inorganic composite porous coating layer.
[0035] The nineteenth aspect of the present disclosure is: in any one of the first to eighteenth aspects, the organic / inorganic composite porous coating is formed by coating a slurry in which a particulate binder polymer and inorganic particles are dispersed in an aqueous dispersion medium on at least one surface of a porous polymer substrate and drying it.
[0036] A twentieth aspect of the present disclosure relates to an electrochemical device, wherein the electrochemical device includes an anode, a cathode, and a separator interposed between the anode and the cathode, wherein the separator is according to any one of the first to nineteenth aspects.
[0037] A twenty-first aspect of the present disclosure is: in the twentieth aspect, the electrochemical device is a lithium secondary battery.
[0038] Beneficial effects
[0039] According to the present disclosure, the organic / inorganic composite porous coating layer of the separator includes acrylic polymer particles and first inorganic particles, wherein the particle size D50(a) of the acrylic polymer particles is in the range of 1 μm to 7 μm, and the particle size D50(b) of the first inorganic particles is in the range of 200 nm to 800 nm, and a / b is 2 to 15. Since the particle size D50 of the acrylic polymer particles is at least twice as large as the particle size D50 of the first inorganic particles, it helps that the inorganic particles of the organic / inorganic composite porous coating layer are less likely to cause damage to the porous polymer substrate even when a high voltage is applied during the lamination process with the electrode, and improves thickness reduction and deformation of the pore structure of the porous polymer substrate.
[0040] Furthermore, according to the present disclosure, the organic / inorganic composite porous coating of the separator comprises hybrid polymer particles of a fluorine-based polymer and an acrylic polymer, and the particle size D50 of the hybrid polymer particles is smaller than the particle size D50 of the acrylic polymer particles. Since the fluorine-based polymer contained in the hybrid polymer particles is insoluble in the electrolyte, the hybrid polymer particles maintain their shape even when immersed in the electrolyte, even if the acrylic polymer is also contained. Therefore, the separator of the present disclosure maintains adhesion to the electrode even in a wet state without significantly losing adhesion to the electrode. On the other hand, the acrylic polymer particles also help maintain the adhesion of the separator to the electrode in a dry state.
[0041] Therefore, in a roll-to-roll continuous process for manufacturing an electrode assembly by laminating an electrode and a separator of the present disclosure, there is an effect of improving dielectric degradation of the separator and improving the shape stability and workability of the electrode assembly. In addition, by using an electrode assembly including the separator to manufacture a battery, a high bonding force can be maintained between the separator and the electrode even in a state soaked with an electrolyte, thereby improving the interface resistance characteristics. In addition, since the binder polymer particles maintain high bonding force in both dry and wet states, the inorganic particles contained in the organic / inorganic composite porous coating do not separate and are well fixed, so that the morphological stability of the separator can be improved. Therefore, there is an effect of improving the thermal stability and dielectric characteristics of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] The accompanying drawings illustrate preferred embodiments of the present disclosure and, together with the detailed description, illustrate the principles of the present disclosure, but the scope of the present disclosure is not limited thereto. On the other hand, the shapes, sizes, proportions, or ratios of the elements in the drawings included in this specification may be exaggerated to emphasize a clearer description.
[0043] Figure 1 is a schematic diagram showing a cross section of a separator according to a specific embodiment of the present disclosure;
[0044] Figure 2 is an SEM image of the surface of the separator of Example 1 before electrolyte impregnation; and
[0045] Figure 3 is a SEM image of a cross section of the separator according to Example 1. DETAILED DESCRIPTION
[0046] The terms or words used in this specification and claims should not be interpreted as conventional meanings or dictionary meanings, but should be interpreted as meanings and concepts that are consistent with the technical concept of the present invention based on the principle that the inventor can appropriately define the concept of the term to describe his invention in the best way. Therefore, since the configurations described in the embodiments described herein are only the most preferred embodiments of the present disclosure and do not represent all technical concepts of the present disclosure, it should be understood that various equivalent solutions and modifications that can replace them may exist at the time of filing this application.
[0047] Figure 1 is a schematic diagram illustrating a cross section of a separator 10 for an electrochemical device according to a specific embodiment of the present disclosure.
[0048] In the present disclosure, the separator 10 includes a porous polymer substrate 1 and an organic / inorganic composite porous coating layer 3 formed on at least one side of the polymer substrate. Figure 1 The organic / inorganic composite porous coating layer 3 is shown to be formed on both surfaces of the polymer substrate 1 , but the organic / inorganic composite porous coating layer 3 may be formed only on one surface of the polymer substrate 1 .
[0049] The organic / inorganic composite porous coating layer 3 includes particulate binder polymers 5 and 7 and first inorganic particles 9. The particulate binder polymers 5 and 7 include hybrid polymer particles 5 and acrylic polymer particles 7 of a fluorine-based polymer and an acrylic polymer.
[0050] like Figure 1As shown, the organic / inorganic composite porous coating 3 contains acrylic polymer particles 7 and first inorganic particles 9, and the particle size D50(a) of the acrylic polymer particles 7 is in the range of 1 μm to 7 μm, the particle size D50(b) of the first inorganic particles 9 is in the range of 200 nm to 800 nm, and a / b is 2 to 15.
[0051] Since the particle size D50 of the acrylic polymer particles 7 is at least twice the particle size D50 of the first inorganic particles 9, it helps that the inorganic particles 9 of the organic / inorganic composite porous coating layer 3 are less likely to damage the porous polymer substrate 1 even when high voltage is applied during the electrode lamination process, and improves the thickness reduction and deformation of the porous polymer substrate 1. If a / b is less than 2, the compression resistance may be insufficient, while if a / b exceeds 15, the resistance may be too high. When the particle size D50(a) of the acrylic polymer particles 7 is less than 1 μm, there is a risk that the adhesion may be reduced, and when the particle size exceeds 7 μm, there is a risk that the resistance may be excessively increased. When the particle size D50(b) of the first inorganic particles 9 is less than 200 nm, the dispersibility in the slurry may be reduced, and when the particle size D50(b) of the first inorganic particles 9 is greater than 800 nm, the thickness of the organic / inorganic composite porous coating layer may be excessively increased or the pores may be too large. In this regard, the particle size D50(a) of the acrylic polymer particles may be 1 μm to 6 μm, more specifically 2 μm to 6 μm, and even more specifically 3 μm to 5 μm. Furthermore, the particle size D50(b) of the first inorganic particles may be in the range of 300 nm to 700 nm, more specifically 400 nm to 600 nm. a / b may be 3 to 13, more specifically 5 to 12, and even more specifically 6 to 11.
[0052] On the other hand, the acrylic polymer particles 7 also contribute to maintaining the adhesion of the separator to the electrodes in a dry state.
[0053] In addition, according to the present disclosure, the organic / inorganic composite porous coating layer 3 of the separator 10 contains hybrid polymer particles 5 of a fluorine-based polymer and an acrylic polymer, and the particle size D50 of the hybrid polymer particles 5 is smaller than the particle size D50 of the acrylic polymer particles 7. Since the fluorine-based polymer contained in the hybrid polymer particles 5 is insoluble in the electrolyte, even if the acrylic polymer is also contained, the hybrid polymer particles 5 maintain their shape even when wetted in the electrolyte. Therefore, the separator 10 of the present disclosure maintains its adhesive force to the electrode even in a wet state without significantly losing its adhesive force to the electrode.
[0054] On the other hand, by adjusting the particle size D50 of the hybrid polymer particles 5 to be smaller than the particle size D50 of the acrylic polymer particles 7, migration to the surface layer is promoted during the coating formation process, as shown in FIG. Figure 1 As shown in FIG. , the organic / inorganic composite porous coating layer 3 has a compositional morphology that is nonuniform in the thickness direction, wherein the content ratio of the hybrid polymer particles 5 / acrylic polymer particles 7 present on the surface portion opposite to the surface in contact with the polymer substrate 1 is greater than the content ratio of the hybrid polymer particles 5 / acrylic polymer particles 7 present within the organic / inorganic composite porous coating layer 3. Therefore, when wetted with an electrolyte, the adhesion of the separator 10 to the electrode can be further improved.
[0055] Therefore, when the hybrid polymer particles 5 and / or the acrylic polymer particles 7 have the above-mentioned form of compositional morphology inhomogeneity in the thickness direction, the polymer particles 5 and 7 are more present on the surface portion opposite to the surface in contact with the polymer substrate 1 than in the interior of the organic / inorganic composite porous coating 3. Therefore, due to the large adhesive properties of the polymer particles present on the surface, the dry / wet adhesive force to the electrode is further increased. In addition, the resistance to external stimuli such as peeling and scratching is increased, and the lamination properties of the electrode are improved. Therefore, very excellent properties can be exhibited during the battery assembly process (e.g., winding and lamination). In addition, since the porosity is improved due to the increase in the inorganic particles toward the interior, excellent ion conductivity properties can be exhibited, thereby contributing to the improvement of battery performance. In this regard, the particle size D50 of the acrylic polymer particles 7 can be 4 to 20 times larger than the particle size D50 of the hybrid polymer particles 5, and the particle size D50 of the hybrid polymer particles 5 can be in the range of 100 nm to 500 nm, but is not limited thereto.
[0056] In addition, the mixing weight ratio of the hybrid polymer particles 5 and the acrylic polymer particles 7 may be 8:2 to 2:8, but is not limited thereto.
[0057] In the specification of the present disclosure, the term "heterogeneity of compositional morphology in the thickness direction, wherein the content ratio of hybrid polymer particles / acrylic polymer particles present on the surface portion opposite to the surface in contact with the polymer substrate is greater than the content ratio of hybrid polymer particles / acrylic polymer particles present in the interior of the organic / inorganic composite porous coating" should be understood to include any aspect if the content ratio of hybrid polymer particles / acrylic polymer particles present on the surface portion opposite to the surface in contact with the polymer substrate of the organic / inorganic composite porous coating is greater than the content ratio of hybrid polymer particles / acrylic polymer particles present under (inside) the surface portion of the porous coating. For example, it should be understood to mean including all of the following: forming the porous coating so that the content ratio of hybrid polymer particles / acrylic polymer particles decreases linearly from the surface of the porous coating to the porous substrate, forming the porous coating so that the content ratio of hybrid polymer particles / acrylic polymer particles decreases nonlinearly from the surface of the porous coating to the porous substrate, and forming the porous coating so that the content ratio of hybrid polymer particles / acrylic polymer particles decreases discontinuously from the surface of the porous coating to the porous substrate, etc.
[0058] The organic / inorganic composite porous coating layer 3 may have a compositional morphology that is non-uniform in the thickness direction, wherein the content of the hybrid polymer particles 5 present on the surface portion opposite to the surface in contact with the polymer substrate 1 is greater than the content of the hybrid polymer particles 5 present inside the organic / inorganic composite porous coating layer 3. Furthermore, the organic / inorganic composite porous coating layer 3 may have a compositional morphology that is non-uniform in the thickness direction, wherein the content of the acrylic polymer particles 7 present on the surface portion opposite to the surface in contact with the polymer substrate 1 is greater than the content of the acrylic polymer particles 7 present inside the organic / inorganic composite porous coating layer 3.
[0059] As described above, in the roll-to-roll continuous process of manufacturing an electrode assembly by laminating the electrode and the separator 10 of the present disclosure, there is an effect of improving the dielectric degradation of the separator 10 and improving the shape stability and workability of the electrode assembly. In addition, since a high bonding force can be maintained between the separator 10 and the electrode even when a battery is manufactured using an electrode assembly including the separator 10 and soaked with an electrolyte, the interface resistance characteristics are improved. In addition, since the binder polymer particles 5 and 7 maintain a high bonding force under both dry conditions and wet conditions, the inorganic particles 9 contained in the organic / inorganic composite porous coating 3 do not separate and are well fixed. Therefore, the shape stability of the separator 10 can be improved. Therefore, there is an effect of improving the thermal stability and dielectric characteristics of the battery.
[0060] According to one embodiment of the present disclosure, the porous polymer substrate 1 can provide a path for the movement of lithium ions while preventing short circuits by electrically insulating the anode and cathode, and can be used without particular limitation as long as it is generally used as a separator polymer substrate for electrochemical devices. As an example of the separator substrate, for example, a porous polymer film or nonwoven fabric containing at least one polymer resin selected from the group consisting of polyolefins such as polyethylene, polyethylene terephthalate, polybutylene terephthalate, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene oxide, polyphenylene sulfide, and polyethylene naphthalate can be used.
[0061] In the present disclosure, the thickness of the polymer substrate may be 3 μm to 50 μm. Although the range of the separator substrate is not particularly limited to the aforementioned range, if the thickness is too thin compared to the above lower limit, the mechanical properties are reduced and the separator may be easily damaged during use of the battery. At the same time, the pore size and porosity present in the separator substrate are not particularly limited, but may be 0.01 μm to 50 μm and 10% to 95% by volume, respectively.
[0062] The organic / inorganic composite porous coating layer 3 is made by mixing a plurality of inorganic particles 9 and particulate binder polymers 5 and 7. Since the polymer substrate 1 is coated with the porous coating layer 3 containing the inorganic particles 9, the heat resistance and mechanical properties of the separator 10 can be further improved. According to a preferred embodiment of the present disclosure, the organic / inorganic composite porous coating layer 3 is provided on both sides of the polymer substrate 1. As described above, by forming the porous coating layer 3 on both sides of the porous substrate 1, the wet adhesion and dry adhesion between the cathode and the separator and between the anode and the separator can be improved.
[0063] The organic / inorganic composite porous coating layer 3 may have a microporous structure due to the interstitial volume between the constituent inorganic particles 9 and the particulate binder polymers 5 and 7. The inorganic particles 9 serve as a spacer capable of maintaining the physical shape of the porous coating layer 3. The interstitial volume refers to a space defined by substantially surface contact with the inorganic particles 9 and the particles of the particulate binder polymers 5 and 7. In addition, since the inorganic particles 9 generally have the property of not changing their physical properties even at high temperatures of 200°C or higher, the separator 10 has excellent heat resistance through the organic / inorganic composite porous coating layer 3. In the present disclosure, the thickness of the organic / inorganic composite porous coating layer 3 may be in the range of 1 μm to 50 μm, 2 μm to 30 μm, or 2 μm to 20 μm, based on the thickness formed on either side of the porous substrate 1.
[0064] In the present disclosure, particulate polymers 5 and 7 refer to binder polymers that are added to the dispersion medium in the form of particles to form the porous coating layer 3 and that maintain the added particle shape after coating and drying, and are distinguished from "non-particulate" binder polymers, which are defined as being formed into a coating layer, whether soluble in the solvent or insoluble in the solvent, and that lose their particle phase during drying and transform into a film-like form. That is, in the present disclosure, "particles" are defined as particles that substantially maintain the same shape as the added particles, and the shape is generally, but not limited to, round particles. In this way, because the polymer particles maintain their granular form, they rarely penetrate into the pores of the porous polymer substrate, thereby helping to improve clogging of the pores of the polymer substrate.
[0065] In one embodiment of the present disclosure, the particulate binder polymers 5 and 7 may be present in an amount of about 90% by weight or more, or about 99% by weight or more, based on the binder component present in the porous coating layer 3. In this specification, the particulate binder polymers 5 and 7 may be referred to as polymer particles, resin particles, or binder particles. The particulate binder polymers 5 and 7 form the porous coating layer 3 having a layered structure through adhesion between the inorganic particles 9 and mutual adhesion between the inorganic particles 9 and the polymer substrate 1.
[0066] The hybrid polymer particles 5 can be prepared with reference to, for example, WO 2020 / 263936, and can be incorporated by reference into the present disclosure.
[0067] The fluorine-based polymer included in the hybrid polymer particles is an electrolyte-insoluble polymer that is a homopolymer of vinylidene fluoride, a copolymer of vinylidene fluoride and other polymerizable monomers, or a mixture of two or more thereof.
[0068] The polymerizable monomer other than vinylidene fluoride may include at least one selected from the group consisting of tetrafluoroethylene, hexafluoropropylene, trifluoroethylene, chlorofluoroethylene, 1,2-difluoroethylene, perfluoro(methyl vinyl) ether, perfluoro(ethyl vinyl) ether, perfluoro(propyl vinyl) ether, perfluoro(1,3-dioxole), perfluoro(2,2-dimethyl-1,3-dioxole), trichloroethylene, and vinyl fluoride, but is not limited thereto. In particular, the fluorine-based polymer may be a copolymer of vinylidene fluoride and hexafluoropropylene. The content of vinylidene fluoride and other polymerizable monomers may be from 1% to 20% by weight of the copolymer, but is not limited thereto.
[0069] In the present disclosure, the comonomer content in PVDF-based polymers can be measured using a Varian 500 MHz 1H-NMR method. For detailed measurement methods, see Journal of Materials Chemistry, 2012, 22, 341 or AMT-3412-0k. For confirmation of NMR spectra, suitable equipment such as a Bruker Avance III HD 700 MHz NMR or a Varian 500 MHz NMR can be used.
[0070] The acrylic polymer constituting the hybrid polymer particles and the acrylic polymer constituting the acrylic polymer particles may each independently include a repeating unit of an alkyl (meth)acrylate having an alkyl group having 1 to 18 carbon atoms, but is not limited thereto.
[0071] In one embodiment of the present disclosure, the Tg of the acrylic polymer included in the hybrid polymer particles may be 10° C. or more lower than the Tg of the acrylic polymer included in the acrylic polymer particles. Since the lower the Tg of the acrylic polymer, the better the adhesion, the lower the Tg of the acrylic polymer included in the hybrid polymer particles, the higher the dry / wet adhesion of the hybrid polymer particles to the electrode.
[0072] More specifically, the Tg of the acrylic polymer contained in the hybrid polymer particles may be 10°C to 30°C, and the Tg of the acrylic polymer contained in the acrylic polymer particles may be 30°C to 50°C. Although the acrylic polymer contained in the hybrid polymer particles has a low Tg, the granular form can be maintained even at room temperature due to the mixed fluorine-based polymer. In addition, when the Tg of the acrylic polymer contained in the acrylic polymer particles is selected to be higher than or equal to room temperature, the particle shape can be maintained at room temperature, thereby exhibiting electrode adhesion during lamination with an electrode.
[0073] The glass transition temperature (Tg) of the acrylic polymer may be 40° C. or lower.
[0074] More specifically, the acrylic polymer includes carboxylic acid ester as a repeating unit, and may preferably be (meth)acrylate. Specific examples of such (meth)acrylates may include, for example, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, hydroxymethyl (meth)acrylate, hydroxyethyl (meth)acrylate, ethylene glycol (meth)acrylate, ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, allyl (meth)acrylate, ethylene di(meth)acrylate, and the like, and may be at least one selected from them. Among these, at least one selected from methyl (meth)acrylate, ethyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate is preferred, and methyl (meth)acrylate is particularly preferred.
[0075] The organic / inorganic composite porous coating layer may include the particulate binder polymer in an amount of 1 wt % to 30 wt % of the organic / inorganic composite porous coating layer, but is not limited thereto.
[0076] The organic / inorganic composite porous coating may further comprise a non-granular acrylic polymer. The non-granular acrylic polymer is an acrylic polymer that is insoluble in an aqueous dispersion medium but does not maintain a granular form, for example, an acrylic polymer having a low Tg of 0°C or lower. The non-granular acrylic polymer may improve the adhesion of the organic / inorganic composite porous coating to the electrode and the bonding between the inorganic particles and between the inorganic particles and the polymer substrate. The non-granular acrylic polymer may be added in an amount of 10 wt% or less based on the total weight of the binder polymer contained in the organic / inorganic composite porous coating, but is not limited thereto.
[0077] Meanwhile, the first inorganic particles contained in the organic / inorganic composite porous coating are not particularly limited as long as they are electrochemically stable. That is, the inorganic particles are not particularly limited as long as they are within the operating voltage range of the applied electrochemical device (e.g., based on Li / Li +It is sufficient that no oxidation reaction and / or reduction reaction occurs at a voltage of 0 V to 5 V. In particular, when using the first inorganic particles having ion transport ability, the performance can be improved by increasing the ionic conductivity in the electrochemical device. In addition, when using inorganic particles having a high dielectric constant as the first inorganic particles, the ionic conductivity of the electrolyte can be improved by promoting an increase in the degree of dissociation of electrolyte salts (such as lithium salts) in the liquid electrolyte.
[0078] For the above reasons, the first inorganic particles may include inorganic particles having a high dielectric constant of 5 or greater or 10 or greater, inorganic particles having lithium ion transport ability, or a mixture thereof. Non-limiting examples of inorganic particles having a dielectric constant of 5 or greater include BaTiO3 alone, Pb(Zr,Ti)O3 (PZT), Pb 1-x La x Zr 1-y Ti y O3 (PLZT, where 0 < x < 1, 0 < y < 1), Pb(Mg 1 / 3 Nb 2 / 3 )O3-PbTiO3 (PMN-PT), hafnium dioxide (HfO2), SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, ZrO2, Y2O3, alumina (Al2O3), boehmite, SiC, TiO2, etc., or a mixture of two or more thereof. In addition, when the above high dielectric constant inorganic particles are mixed with inorganic particles having lithium ion transport ability, their synergistic effect can be doubled.
[0079] Non-limiting examples of inorganic particles having lithium ion transport ability include lithium phosphate (Li3PO4), lithium titanium phosphate (Li x Ti y (PO4)3, 0 < x < 2, 0 < y < 3), lithium aluminum titanium phosphate (Li x Al y Ti z )(PO4)3, 0 < x < 2, 0 < y < 1, 0 < z < 3), based on (LiAlTiP) x O y of glass (0 < x < 4, 0 < y < 13) such as 14Li2O-9Al2O3-38TiO2-39P2O5, lithium lanthanum titanate (Li x La y TiO3, 0 < x < 2, 0 < y < 3), lithium germanium thiophosphate (Li x Ge y P z S w , 0 < x < 4, 0 < y < 1, 0 < z < 1, 0 < w < 5) such as Li 3.25Ge 0.25 P 0.75 S4 etc., lithium nitrides (Li x N y , 0 < x < 4, 0 < y < 2) such as Li3N, SiS2-based glasses (Li x Si y S z , 0 < x < 3, 0 < y < 2, 0 < z < 4) such as Li3PO4-Li2S-SiS2, P2S5-based glasses (Li x P y S z , 0 < x < 3, 0 < y < 3, 0 < z < 7) such as LiI-Li2S-P2S5 etc., or mixtures thereof.
[0080] Meanwhile, the organic / inorganic composite porous coating may further include second inorganic particles having a particle size D50 smaller than the particle size D50 of the first inorganic particles and different from the first inorganic particles. By mixing these second inorganic particles, the packing density of the porous coating can be improved, thereby further improving the heat resistance. In this regard, the particle size D50 of the second inorganic particles may be in the range of 100 nm to 500 nm. <00...........
[0081] As the second inorganic particles, the above-mentioned first inorganic particles can be used. In particular, alumina can be used as the first inorganic particle, and boehmite can be used as the second inorganic particle.
[0082] In the organic / inorganic composite porous coating, the content ratio of the inorganic particles is determined in consideration of the thickness, pore size, and porosity of the finally prepared organic / inorganic composite porous coating, but based on 100% by weight of the porous coating, the inorganic particles may be included in the range of 70% to 99% by weight. When the content of the inorganic particles is less than 70% by weight, the heat resistance may decrease. On the other hand, when the content of the inorganic particles is too large, the amount of the binder is relatively small, and thus the adhesion of the porous coating may decrease.
[0083] On the other hand, in one embodiment of the present disclosure, the separator including the organic / inorganic composite porous coating can be prepared by: mixing binder particles and inorganic particles with an aqueous dispersion medium to prepare a slurry for forming a coating, and then coating the slurry on at least one surface of a polymer substrate.
[0084] As the coating method, dip coating, die coating, roll coating, comma coating, or a mixture thereof can be adopted.
[0085] In one embodiment of the present disclosure, the aqueous dispersion medium can comprise water and at least one of the alcohol with 1 to 5 carbon atoms. For example, the aqueous dispersion medium can comprise a mixture of water and isopropyl alcohol. In the above-mentioned production method, by using an aqueous dispersion medium, the binder particles are dispersed while maintaining particle shape in the aqueous dispersion medium, and are not dissolved in the dispersion medium. For this reason, the binder particles can maintain particle state in the prepared organic / inorganic composite porous coating, and do not enter the pores of the polymer substrate.
[0086] On the other hand, in one embodiment of the present disclosure, the slurry used to form the coating is preferably controlled so that the solid concentration (excluding the dispersion medium) is in the range of 20% to 50% by weight. By controlling the solid concentration, average particle size, and content ratio of the injected binder particles within the above ranges, it is advantageous to obtain the separator of the present disclosure having an organic / inorganic composite porous coating with a heterogeneous compositional morphology.
[0087] On the other hand, the separator of the present disclosure can be applied to an electrochemical device. The electrochemical device may include an anode and a cathode, and the separator may be inserted between the anode and the cathode. The electrochemical device includes all devices that perform electrochemical reactions, and specific examples thereof include all types of primary batteries, secondary batteries, fuel cells, solar cells, or capacitors. In particular, lithium ion secondary batteries in secondary batteries are preferred: including lithium metal secondary batteries, lithium ion secondary batteries, lithium polymer secondary batteries, or lithium ion polymer secondary batteries.
[0088] In a specific embodiment, according to the present disclosure, an electrochemical device can be manufactured according to conventional methods known in the art. According to one embodiment of the present disclosure, an electrochemical device can be configured by inserting the above separator between a cathode and an anode.
[0089] That is, the separator prepared by the above method is inserted between the anode and the cathode, and the electrode assembly is manufactured by applying heat and / or pressure to combine the separator lamination process. In one embodiment of the present disclosure, the lamination process can be carried out by a rolling device including a pair of pressure rollers. That is, the anode, separator and cathode are stacked sequentially and placed between the pressure rollers to achieve interlayer bonding. In this case, the lamination process can be carried out by a hot pressing method.
[0090] The electrochemical device can be manufactured by housing an electrode assembly assembled by laminating an anode, a separator, and a cathode in a battery case, and then injecting an electrolyte.
[0091] In one embodiment of the present disclosure, the electrode is not particularly limited, and the electrode active material can be prepared in a form adhered to an electrode current collector according to conventional methods known in the art. As a non-limiting example of the cathode active material in the electrode active material, a conventional cathode active material that can be used for the cathode of a conventional electrochemical device can be used, and in particular, lithium manganese oxide, lithium cobalt oxide, lithium nickel oxide, lithium iron oxide, or a lithium intercalation material such as a composite oxide formed by a combination thereof is preferred. As a non-limiting example of the anode active material, a conventional anode active material that can be used for the anode of a conventional electrochemical device can be used. And in particular, lithium metal or lithium alloy is preferred; lithium adsorption materials such as carbon, petroleum coke, activated carbon, graphite or other carbon. Non-limiting examples of cathode current collectors include foils made of aluminum, nickel, or a combination thereof, and non-limiting examples of anode current collectors include foils made of copper, gold, nickel, or a copper alloy, or a combination thereof.
[0092] The electrolyte solution that can be used in the present disclosure is an electrolyte having + B - Salts of the same structure, and A + including ions formed from alkali metal cations such as Li + 、Na + , K + , or a combination thereof, or B - Including PF6 - 、BF4 - 、Cl - Br - , I - 、ClO4 - 、AsF6 - 、CH3CO2 - CF3SO3 - 、N(CF3SO2)2 - 、C(CF2SO2)3 - , or a combination thereof. In the electrolyte, the salt may be dissolved or dissociated in an organic solvent including, but not limited to, propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), and gamma butyrolactone (γ-butyrolactone) or a mixture thereof.
[0093] Depending on the manufacturing process and desired physical properties of the final product, electrolyte injection can be performed at an appropriate stage in the battery manufacturing process. That is, the electrolyte can be applied before or in the final stage of battery assembly. As a method for applying the electrode assembly of the present disclosure to a battery, in addition to the general winding method, a method of laminating, stacking, and folding separators and electrodes is also possible.
[0094] Embodiments of the invention
[0095] Hereinafter, examples will be given to describe the present disclosure in detail. However, embodiments according to the present disclosure may be modified in various other forms, and the scope of the present disclosure should not be interpreted as being limited to the embodiments described below. The embodiments of the present disclosure are provided to more fully illustrate the present disclosure to those of ordinary skill in the art.
[0096] Example 1
[0097] 8.2 parts by weight of hybrid polymer particles [Arkema, LBG4330LX, D50: 300 nm, hybrid polymer particles in which a copolymer of VDF and HFP polymerized in a weight ratio of 95:5 and a copolymer of ethyl acrylate and methyl methacrylate (Tg 20°C) in a weight ratio of 7:3], 8.2 parts by weight of acrylic polymer particles [D50: 5 μm, a copolymer of styrene and butyl acrylate (Tg 40°C)], and 80 parts by weight of inorganic particles (Al2O3, D50: 500 nm) were added to water and dispersed to prepare a dispersion for forming a porous coating layer (solid concentration of 35 wt%).
[0098] Next, a polyethylene separator substrate (porosity 40%, thickness 9 μm) was prepared. The dispersion was applied to both sides of the separator substrate by bar coating using a doctor blade, and then dried with hot air at 50°C using a heat gun to form a porous coating layer having a thickness of 12 μm per side. The particle size D50 of the acrylic polymer particles / the particle size D50 of the first inorganic Al2O3 particles (a / b) was 10.
[0099] Figure 2 is an SEM image of the surface of the separator of Example 1 before being impregnated with the electrolyte, and Figure 3 is a SEM image of a cross section of the separator according to Example 1.
[0100] Example 2
[0101] A porous coating layer was formed in the same manner as in Example 1, except that the content of the hybrid polymer particles was 10.2 parts by weight, the content of the acrylic polymer particles was 10.2 parts by weight, and the content of the inorganic particles was changed to 75 parts by weight to prepare a dispersion for forming a porous coating layer (solid concentration of 35% by weight). The particle size D50 of the acrylic polymer particles / the particle size D50 of the first inorganic particles Al2O3 (a / b) was 10.
[0102] Example 3
[0103] A porous coating layer was formed in the same manner as in Example 1, except that 0.9 parts by weight of a non-granular acrylic polymer [Toyochem CSB130, particle size 150 nm, Tg -30°C] was added to water based on the solid content. The ratio (a / b) of the particle size D50 of the acrylic polymer particles / the particle size D50 of the first inorganic Al2O3 particles was 10.
[0104] Example 4
[0105] A porous coating layer was formed in the same manner as in Example 1, except that 80 parts by weight of inorganic particles (Al2O3, D50: 500 nm) and boehmite (D50: 300 nm) were added in a weight ratio of 85:15 instead of 80 parts by weight of the inorganic particles (Al2O3, D50: 500 nm). The particle size D50 of the acrylic polymer particles / the particle size D50 of the first inorganic particles Al2O3 (a / b) was 10.
[0106] Comparative Example 1
[0107] A porous coating layer was formed in the same manner as in Example 1, except that the dispersion for forming the porous coating layer (35% by weight solid concentration) was prepared by changing the content of the acrylic polymer particles to 16.4 parts by weight without adding the hybrid polymer particles. The particle size D50 of the acrylic polymer particles / the particle size D50 of the first inorganic Al2O3 particles (a / b) was 10.
[0108] Comparative Example 2
[0109] A porous coating layer was formed in the same manner as in Example 1, except that the dispersion for forming the porous coating layer (35 wt% solid concentration) was prepared by changing the content of the hybrid polymer particles to 16.4 parts by weight without adding the acrylic polymer particles. The particle size D50 of the acrylic polymer particles / the particle size D50 of the first inorganic particles Al2O3 (a / b) was 0.
[0110] Comparative Example 3
[0111] A porous coating layer was formed in the same manner as in Example 1, except that 8.2 parts by weight of acrylic polymer particles having a small particle size D50 [a copolymer of styrene and butyl acrylate (Tg 40° C.) (D50: 0.9 μm)] were added instead of 8.2 parts by weight of the acrylic polymer particles having a D50 of 5 μm in Example 1. The ratio (a / b) of the particle size D50 of the acrylic polymer particles / the particle size D50 of the first inorganic particles Al 2 O 3 was 1.8.
[0112] Comparative Example 4
[0113] A porous coating layer was formed in the same manner as in Example 1, except that 8.2 parts by weight of acrylic polymer particles having a small particle size D50 [a copolymer of styrene and butyl acrylate (Tg 40° C.) (D50: 0.4 μm)] were added instead of 8.2 parts by weight of the acrylic polymer particles having a D50 of 5 μm in Example 1. The ratio (a / b) of the particle size D50 of the acrylic polymer particles / the particle size D50 of the first inorganic particles Al 2 O 3 was 0.8.
[0114] Measurement of average particle size D50
[0115] D50 may be defined as the particle size based on 50% of the particle size distribution and is measured using a laser diffraction method.
[0116] Measurement of Tg
[0117] The Tg of 25 mg of the sample was measured using DSC in a nitrogen atmosphere at a temperature increase rate of 10°C / min over a range from room temperature to 300°C.
[0118] Wet bond specimen production
[0119] The separators and cathodes obtained in each example and comparative example were laminated, immersed in 1.0 g of electrolyte (ethylene carbonate:ethyl methyl carbonate content ratio = 7:3, LiPF6 1M), and left at room temperature for 24 hours. Thereafter, a sample was prepared by lamination using a hot press. At this time, pressurization was performed at 70°C and 5 kgf for 5 minutes. The sample size was 2 cm × 6 cm.
[0120] The cathode was prepared as follows. 0.8 Co 0.1 Mn 0.1 O2, PVdF, and carbon black were mixed and dispersed in 2-methyl-2-pyrrolidone at a weight ratio of 97.0:1.5:1.5 to prepare a cathode slurry, coated on an aluminum current collector, and then dried and roll-pressed to prepare a cathode.
[0121] Dry bonded specimen production
[0122] The separators and anodes obtained in each example and comparative example were laminated using a hot press to prepare a sample. Pressing was performed at 60° C. for 1 second at 6.5 MPa. The sample size was 2.5 cm×6 cm.
[0123] The anode was prepared as follows: Graphite, SBR, and CMC were mixed and dispersed in distilled water at a weight ratio of 89.2:10:0.8 to prepare an anode slurry, which was coated on a copper current collector, dried, and roll-pressed to prepare an anode.
[0124] Measurement of adhesion to electrodes
[0125] Using each sample prepared above, the wet adhesion and dry adhesion of the separator were evaluated, and the results are summarized in Table 1 below. After preparing each sample, the sample was left at room temperature for 1 hour and then the adhesion was measured. Adhesion was measured using a tensile testing machine (UTM equipment) by peeling at an angle of 180 ° (for dry) and 90 ° (for wet).
[0126] [Table 1]
[0127]
[0128] As can be seen in Table 1, in Comparative Example 1, the dry adhesion is high and the wet adhesion is low, so when applied to an actual battery, the battery performance may deteriorate. Comparative Example 2 has a problem in that since the dry adhesion is low, the adhesion is reduced during the electrode assembly manufacturing process. Comparative Examples 3 and 4 have low compression resistance, so the thickness of the porous polymer substrate may be reduced due to the high pressure applied when the separator and the electrode are laminated, and thus the dielectric properties of the separator may be deteriorated, such as deformation of the pore structure. On the other hand, according to the embodiment, the separator exhibits good levels of wet adhesion and dry adhesion, thereby exhibiting excellent electrochemical effects in the electrode assembly manufacturing process and battery operation.
[0129] [Explanation of Reference Numerals]
[0130] 1: Polymer substrate
[0131] 3: Organic / inorganic composite porous coating
[0132] 5: Hybrid polymer particles
[0133] 7: Acrylic polymer particles
[0134] 9: Inorganic particles
[0135] 10: Separator
Claims
1. An electrochemical device separator, comprising a porous polymer substrate and an organic / inorganic composite porous coating formed on at least one side of the polymer substrate, wherein the organic / inorganic composite porous coating comprises a particulate binder polymer and first inorganic particles, The particulate binder polymer comprises hybrid polymer particles of a fluorine-based polymer and an acrylic polymer and acrylic polymer particles, The particle size D50 "a" of the acrylic polymer particles is in the range of 1 μm to 7 μm, The particle size D50 "b" of the first inorganic particles is in the range of 200 nm to 800 nm, a / b is 2 to 15, and The particle size D50 of the hybrid polymer particles is smaller than the particle size D50 of the acrylic polymer particles. 2 . The separator according to claim 1 , wherein the particle size D50 “a” of the acrylic polymer particles is in the range of 2 μm to 6 μm, and the particle size D50 “b” of the first inorganic particles is in the range of 300 nm to 700 nm, and a / b is 5 to 12. 3 . The separator according to claim 1 , wherein a particle size D50 of the acrylic polymer particles is 4 to 20 times larger than a particle size D50 of the hybrid polymer particles. 4 . The separator according to claim 1 , wherein a particle size D50 of the hybrid polymer particles is in the range of 100 nm to 500 nm. 5 . The separator according to claim 1 , wherein the hybrid polymer particles and the acrylic polymer particles are mixed in a weight ratio of 8:2 to 2:
8. 6 . The separator according to claim 1 , wherein a glass transition temperature Tg of the acrylic polymer included in the hybrid polymer particles is lower than Tg of the acrylic polymer included in the acrylic polymer particles by 10° C. or more. 7 . The separator according to claim 6 , wherein Tg of the acrylic polymer contained in the hybrid polymer particles is in the range of 10° C. to 30° C., and Tg of the acrylic polymer contained in the acrylic polymer particles is in the range of 30° C. to 50° C. 8 . The separator according to claim 1 , wherein the fluorine-based polymer is a homopolymer of vinylidene fluoride, a copolymer of vinylidene fluoride and other polymerizable monomers, or a mixture of two or more thereof.
9. The separator according to claim 8, wherein the monomer comprises at least one selected from the group consisting of tetrafluoroethylene, hexafluoropropylene, trifluoroethylene, chlorofluoroethylene, 1,2-difluoroethylene, perfluoro(methyl vinyl) ether, perfluoro(ethyl vinyl) ether, perfluoro(propyl vinyl) ether, perfluoro(1,3 dioxole), perfluoro(2,2-dimethyl-1,3-dioxole), trichloroethylene and vinyl fluoride. 10 . The separator according to claim 8 , wherein the fluorine-based polymer is a copolymer of vinylidene fluoride and hexafluoropropylene. 11 . The separator according to claim 8 , wherein the content of the monomer is 1 to 20 wt % of the copolymer. 12 . The separator according to claim 1 , wherein the acrylic polymer constituting the hybrid polymer particles and the acrylic polymer constituting the acrylic polymer particles each independently contain a repeating unit of an alkyl (meth)acrylate having an alkyl group having 1 to 18 carbon atoms. 13 . The separator according to claim 1 , wherein the organic / inorganic composite porous coating further comprises a non-particulate acrylic polymer. 14 . The separator according to claim 13 , wherein the non-particulate acrylic polymer has a Tg of 0° C. or less.
15. The separator according to claim 1, wherein the organic / inorganic composite porous coating layer comprises second inorganic particles different from the first inorganic particles, and The particle size D50 of the second inorganic particles is smaller than the particle size D50 of the first inorganic particles. 16 . The separator according to claim 15 , wherein a particle size D50 of the second inorganic particles is in the range of 100 μm to 500 μm. 17 . The separator according to claim 15 , wherein the first inorganic particles are alumina, and the second inorganic particles are boehmite. 18 . The separator according to claim 1 , wherein the organic / inorganic composite porous coating layer comprises the particulate binder polymer in an amount of 1 wt % to 30 wt % based on the total weight of the organic / inorganic composite porous coating layer.
19. The separator according to claim 1, wherein the organic / inorganic composite porous coating layer is formed by coating and drying a slurry in which the particulate binder polymer and the inorganic particles are dispersed in an aqueous dispersion medium on at least one surface of the porous polymer substrate. 20 . An electrochemical device comprising an anode, a cathode, and a separator interposed between the anode and the cathode, wherein the separator is the separator according to any one of claims 1 to 19 .
21. The electrochemical device according to claim 20, wherein the electrochemical device is a lithium secondary battery.
Citation Information
Patent Citations
Separator having porous coating layer and electrochemical device containing the same
CN101960659A
Method for manufacturing a polymer electrolyte separator and polymer electrolyte separator therefrom
CN104039874A
Separator provided with electrode bonding layer, and electrochemical device comprising same
CN108352482A
Separator and electrochemical device including same
CN110521023A
Lithium ion battery separator
CN111492507A