Defoaming agent for fermentation and preparation method thereof

By synthesizing silicon grease with low viscosity and high hydroxyl content with hydroxy silicone oil and hydrophobic silica, and combining it with GP-type glycerol polyether and polyether modified silicone, the problem of poor stability of existing defoaming agents at high temperatures is solved. , achieves efficient defoaming and foam suppression effects, and is suitable for foam removal during microbial fermentation.

CN118925299APending Publication Date: 2024-11-12NANJING ZIYIJIE TECH R&D CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411329925.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing defoaming agents have poor stability in high temperature environments, with more silicon residues, poor foam suppression effect, and it is difficult to effectively remove foam during microbial fermentation, affecting fermentation efficiency.

Method used

The hydroxy silicone oil with low viscosity and high hydroxyl content is synthesized with hydrophobic silica, and combined with GP-type glycerol polyether and polyether modified silicone, emulsified using emulsifiers and isomerized alcohol polyoxyethylene ether. Thickening agent and bactericide are added to prepare a fermentation defoaming agent with excellent defoaming and antifoaming effects.

Benefits of technology

It achieves defoaming and foaming inhibiting effects with good stability at high temperatures, reduces silicon residues, is suitable for various bacterial species, can automatically restore the emulsion state, and improves fermentation efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005056542670000021
    Figure BDA0005056542670000021
  • Figure BDA0005056542670000031
    Figure BDA0005056542670000031
  • Figure BDA0005056542670000041
    Figure BDA0005056542670000041
Patent Text Reader

Abstract

The invention discloses a defoaming agent for fermentation, which is prepared from the following ingredients in parts by weight: 120 to 150 parts of hydroxyl silicone oil, 5 to 8 parts of hydrophobic silicon dioxide, 100 to 125 parts of GP type glyceryl polyether, 40 to 60 parts of polyether modified organic silicon, 40 to 60 parts of emulsifying agents, 20 to 25 parts of isomeric alcohol polyoxyethylene ether, 15 to 18 parts of thickening agents, 2 to 5 parts of sterilizing agents and 580 to 650 parts of deionized water. Compared with the prior art, the hydroxyl silicone oil with low viscosity and high hydroxyl content and the hydrophobic silicon dioxide are selected to prepare the silicone grease, the obtained silicone grease is low in viscosity and easy to emulsify and has a good foam eliminating and inhibiting effect in fermentation liquor, the polyether modified organic silicon is further added and has good compatibility with the silicone grease and the GP type glyceryl polyether, and the silicone grease is suitable for various strains and has a good foam eliminating and inhibiting effect. The emulsion has self-emulsifying property and can automatically recover the emulsion state after high-temperature sterilization. The defoaming agent disclosed by the invention has excellent defoaming and foam-inhibiting performance, good water dispersibility and good stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a defoamer for fermentation and a preparation method thereof, belonging to the technical field of foam control. Background Art

[0002] Microbial fermentation technology is widely used in the industrial field, including pharmaceutical industry, food industry, energy industry, chemical industry, agriculture and environmental protection. However, during the microbial fermentation process, due to ventilation and stirring and the respiration of microorganisms, a large amount of foam is usually generated in the fermentation tank. The foam will carry away a large amount of fermentation liquid, and will also pollute the environment and affect the normal operation of fermentation. The formation of foam is mainly formed by the interaction of air, carbon dioxide and some colloidal substances such as proteins and sugars. These small bubbles form a large amount of foam due to the accumulation of time. At the same time, a layer of liquid film is formed between the bubbles. The smaller the bubble, the more liquid film there is, and the more fermentation liquid is entrained, making the fermentation efficiency extremely low.

[0003] At present, the foam in the fermentation process is mainly eliminated by adding defoamers, which are usually added by the flow addition method or the base material method, and the types of defoamers added are mainly silicone and polyether defoamers. Silicone defoamers usually have excellent defoaming performance due to their low surface tension. However, silicone defoamers are easy to demulsify under high temperature conditions and it is difficult to achieve the desired effect. The temperature of high-temperature sterilization basically reaches 130°C. After high-temperature sterilization, it is easy to precipitate, and there is silicon residue, which greatly reduces the defoaming and anti-foaming effect. Polyether defoamers are mainly glycerol ether GP and GPE, etc., which have the characteristic of no residue. Among them, GP type polyether defoamer has poor hydrophilicity, low solubility in the system, good anti-foaming effect, but poor defoaming effect. Although GPE type polyether defoamer has good hydrophilicity, high solubility in the system and good defoaming effect, it has a short anti-foaming time. At the same time, the defoaming and anti-foaming effects of polyether defoamers are affected by temperature. The defoaming and anti-foaming effects will be greatly attenuated at high temperature. The effect is not as good as silicone defoamer, and the addition amount is large. There are also some defoamers on the market that are compounded from silicone defoamers and polyether defoamers. However, polyether defoamers and silicone defoamers are not compatible with each other. Therefore, the compounded products often have poor stability at room temperature, and a large amount of precipitation will occur after high-temperature sterilization, making it difficult to ensure the defoaming and anti-foaming effect. Summary of the invention

[0004] The purpose of the present invention is to solve the deficiencies of the above-mentioned prior art and to provide a defoamer for fermentation and a preparation method thereof. The defoamer has excellent defoaming and defoaming performance, good water dispersibility, good stability, less precipitation and low silicon residue.

[0005] In order to achieve the above object, the present invention adopts the following technical solution:

[0006] A fermentation defoamer, comprising the following components in parts by weight:

[0007] Hydroxy silicone oil 120-150 parts

[0008] 5-8 parts of hydrophobic silica

[0009]

[0010] Furthermore, the average molecular weight of the hydroxy silicone oil is 100-300, the hydroxy content is 2%-6%, and the viscosity at 25° C. is 50-300 cs.

[0011] Furthermore, the specific surface area of ​​the hydrophobic silica is 300 to 500 m 2 / g.

[0012] Furthermore, the polyether-modified silicone is prepared by hydrogenated silicone oil and allyl polyether through hydrosilylation, and has a viscosity of 500 to 3000 cs at 25°C.

[0013] Furthermore, the emulsifier is one of Span-40, Span-60, Tween-40 or Tween-60, or a combination of two or more in any proportion.

[0014] Furthermore, the isomeric alcohol polyoxyethylene ether is one of isomeric decanol polyoxyethylene ether, isomeric undecanol polyoxyethylene ether or isomeric tridecanol polyoxyethylene ether.

[0015] Furthermore, the thickener is an alkali swelling thickener, which can be purchased from the market, such as ASE-60 from Dow Chemical; the bactericide used is kasone or s-triazine.

[0016] The preparation method of the above-mentioned fermentation defoamer comprises the following steps:

[0017] (1) putting hydroxy silicone oil and hydrophobic silica into a container in sequence, stirring and mixing, heating to 110-150° C., and stirring for 1-3 hours to obtain silicone grease;

[0018] (2) putting the silicone grease prepared in step (1) with glycerol polyether, polyether-modified silicone, emulsifier, and isomeric alcohol polyoxyethylene ether into a container, stirring and mixing, heating to 70° C., and stirring for 0.5 to 2 hours to obtain a mixture;

[0019] (3) Add the thickener to deionized water, stir evenly, and adjust the pH to 7-8 to obtain thickened water, and add the thickened water in batches to the mixture obtained in step (2), maintain the temperature of the mixed system at 60-70° C., stir and emulsify, stop heating after the emulsion phase transition, add the remaining thickening water, continue stirring, and add the fungicide after the temperature of the mixed system drops to 35-40° C., mix evenly, and obtain a fermentation defoaming agent.

[0020] Furthermore, in step (3), the stirring speed of the stirring emulsification is 180 to 300 rpm.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1) The present invention uses low-viscosity, high-hydroxyl content hydroxy silicone oil and hydrophobic silica to prepare silicone grease. The prepared silicone grease has low viscosity and is easy to emulsify. The condensation reaction between the hydroxyl groups forms a cross-linked structure, so that the silicone grease has a good anti-foaming effect during fermentation.

[0023] 2) The present invention uses GP type glycerol polyether, which has good lipophilicity and good anti-foaming effect. After being mixed with silicone grease, it participates in emulsification and has excellent defoaming and anti-foaming effects.

[0024] 3) The present invention adds polyether-modified silicone as an active substance to participate in emulsification, has good compatibility with silicone grease and GP-type glycerol polyether, can be applied to various strains, has self-emulsification, and can automatically restore to an emulsion state after high-temperature sterilization.

[0025] 4) The present invention uses Span and Tween as emulsifiers, which are synergistically emulsified with isomeric alcohol polyoxyethylene ether. The amount of emulsifier used is small, the emulsifying power is strong, the finished emulsion has good stability and high temperature resistance, and no precipitation occurs after high temperature sterilization. DETAILED DESCRIPTION

[0026] The technical solution of the present invention is clearly and completely described below in conjunction with specific embodiments.

[0027] It should be noted that in the following examples, the viscosity of the hydroxy silicone oil used is 100 cs, the hydroxy content is 4%; the specific surface area of ​​the hydrophobic silica used is 350 m 2 / g; the GP type glycerol polyether used was purchased from Jiangsu Lihong Technology Development Co., Ltd.; the polyether modified silicone with a viscosity of 2500cs was purchased from Changzhou Renjie New Material Technology Co., Ltd.; the thickener used was ASE-60, purchased from Dow Chemical, but are not limited thereto.

[0028] Example 1

[0029] A fermentation defoamer, comprising the following components in parts by weight:

[0030]

[0031] The preparation method of the above fermentation defoamer:

[0032] (1) Adding hydroxy silicone oil and hydrophobic silica into a container in sequence, stirring and mixing, heating to 110° C., and continuing to keep the temperature and stir for 2 hours to obtain silicone grease;

[0033] (2) putting the silicone grease prepared in step (1), GP type glycerol polyether, polyether-modified silicone, emulsifier (composed of Span-60 and Tween-60 in a mass ratio of 1:1), and isomeric alcohol polyoxyethylene ether into a container, stirring and mixing, and heating to 70° C., and continuing to keep warm and stir for 1 hour to obtain a mixture;

[0034] (3) Add the thickener to deionized water, stir evenly, and adjust the pH to 7-8 to obtain thickened water, and add the thickened water in batches to the mixture obtained in step (2), maintain the temperature of the mixed system at 60-65° C., stir and emulsify at a speed of 240 rpm, stop heating after the emulsion phase transition, add the remaining thickening water, continue stirring, and add the fungicide after the temperature of the mixed system drops to 35-40° C., mix evenly, and obtain a fermentation defoaming agent.

[0035] Example 2

[0036] A fermentation defoamer, comprising the following components in parts by weight:

[0037]

[0038] The preparation method of the above fermentation defoamer:

[0039] (1) Adding hydroxy silicone oil and hydrophobic silica into a container in sequence, stirring and mixing, heating to 110° C., and continuing to keep the temperature and stir for 2 hours to obtain silicone grease;

[0040] (2) putting the silicone grease prepared in step (1), GP type glycerol polyether, polyether-modified silicone, emulsifier (composed of Span-60 and Tween-60 in a mass ratio of 1:1), and isomeric alcohol polyoxyethylene ether into a container, stirring and mixing, and heating to 70° C., and continuing to keep warm and stir for 1 hour to obtain a mixture;

[0041] (3) Add the thickener to deionized water, stir evenly, and adjust the pH to 7-8 to obtain thickened water, and add the thickened water in batches to the mixture obtained in step (2), maintain the temperature of the mixed system at 60-65° C., stir and emulsify at a speed of 240 rpm, stop heating after the emulsion phase transition, add the remaining thickening water, continue stirring, and add the fungicide after the temperature of the mixed system drops to 35-40° C., mix evenly, and obtain a fermentation defoaming agent.

[0042] Example 3

[0043] A fermentation defoamer, comprising the following components in parts by weight:

[0044]

[0045]

[0046] The preparation method of the above fermentation defoamer:

[0047] (1) Add hydroxy silicone oil and hydrophobic silica into a container in sequence, stir and mix, heat to 110° C., and continue to keep warm and stir for 2 hours to obtain silicone grease;

[0048] (2) putting the silicone grease prepared in step (1), GP type glycerol polyether, polyether-modified silicone, emulsifier (composed of Span-60 and Tween-60 in a mass ratio of 1:1) and isomeric alcohol polyoxyethylene ether into a container, stirring and mixing, heating to 70° C., and continuing to keep warm and stir for 1 hour to obtain a mixture;

[0049] (3) Add the thickener to deionized water, stir evenly, and adjust the pH to 7-8 to obtain thickened water, and add the thickened water in batches to the mixture obtained in step (2), maintain the temperature of the mixed system at 60-65° C., stir and emulsify at a speed of 240 rpm, stop heating after the emulsion phase transition, add the remaining thickening water, continue stirring, and add the fungicide after the temperature of the mixed system drops to 35-40° C., mix evenly, and obtain a fermentation defoaming agent.

[0050] Performance Testing:

[0051] The defoaming performance and foam suppression performance of the defoaming agents prepared in Examples 1-3 were tested, and an imported polyether GPE defoamer, a domestic GPE polyether defoamer, and a domestic silicone defoamer were used as control samples for testing and comparison. Bacillus subtilis fermentation broth was used as the test base liquid, and the Bacillus subtilis fermentation broth fermented to a foaming period of about 6-10 hours was taken as the foaming liquid for testing. The test method was based on the test method in 5.5 Defoaming Performance (Defoaming Time) Determination and 5.6 Defoaming Suppression Performance (Foam Volume) Determination in GB / T 26527-2011.

[0052] 1) First, connect the autoclave through the steam generator, dilute the defoamer ten times with water and place it in the autoclave, turn on the steam generator for sterilization for half an hour, observe the state of the diluted liquid, and confirm that there is no precipitation;

[0053] 2) Defoaming performance test: 50 g of Bacillus subtilis fermentation liquid in the fermentation cycle was placed in a 100 mL stoppered measuring cylinder, 0.3 g of sterilized defoaming agent diluent was added, the bottle cap was covered and shaken evenly, the measuring cylinder was vertically shaken up and down 10 times and 100 times at a frequency of 2 times / s and an amplitude of (30-35) cm. After standing, a stopwatch was used to record the time for the foam to disappear to the liquid surface, in seconds. The test results are shown in Table 1.

[0054] 3) Antifoaming performance test: 200 g of Bacillus subtilis fermentation liquid in the fermentation cycle was placed in a 1000 mL measuring cylinder, 0.3 g of sterilized defoaming agent diluent was added, and the mixture was shaken evenly. The air blower was turned on, the flow rate was adjusted to 300 L / h, and the air blower head was placed in the measuring cylinder. The time for the foam to rise to 1 L was recorded in min. The test results are shown in Table 2.

[0055] Table 1 Defoaming performance test results

[0056]

[0057] Table 2 Antifoaming performance test results

[0058]

[0059] It can be seen from the test results of Table 1 and Table 2 that, compared with the imported GPE polyether defoamers, domestic GPE polyether defoamers and domestic silicone defoamers commonly used in the art, the defoamers prepared in Examples 1-3 of the present invention have better defoaming performance and antifoaming performance in Bacillus subtilis fermentation broth.

Claims

1. A fermentation defoamer, characterized in that: Contains the following ingredients by weight:

2. The fermentation defoamer according to claim 1, wherein The average molecular weight of the hydroxy silicone oil is 100-300, the hydroxy content is 2%-6%, and the viscosity is 50-300cs at 25°C.

3. The fermentation defoamer according to claim 1, wherein The specific surface area of ​​the hydrophobic silica is 300 to 500 m 2 / g.

4. The fermentation defoamer according to claim 1, wherein The viscosity of the polyether-modified silicone at 25° C. is 500 to 3000 cs.

5. The fermentation defoamer according to claim 1, characterized in that The emulsifier is one of Span-40, Span-60, Tween-40 or Tween-60, or a combination of two or more of them in any proportion.

6. The fermentation defoamer according to claim 1, characterized in that The isomeric alcohol polyoxyethylene ether is one of isomeric decanol polyoxyethylene ether, isomeric undecanol polyoxyethylene ether or isomeric tridecanol polyoxyethylene ether.

7. The fermentation defoamer according to any one of claims 1 to 6, characterized in that The thickener is an alkali swelling thickener.

8. The method for preparing the fermentation defoamer according to any one of claims 1 to 7, characterized in that: The steps include: (1) putting hydroxy silicone oil and hydrophobic silica into a container in sequence, stirring and mixing, heating to 110-150° C., and stirring for 1-3 hours to obtain silicone grease; (2) putting the silicone grease prepared in step (1) into a container with glycerol polyether, polyether-modified silicone, emulsifier, and isomeric alcohol polyoxyethylene ether, stirring and mixing, heating to 70° C., and stirring for 0.5 to 2 hours to obtain a mixture; (3) Add the thickener to deionized water, stir evenly, and adjust the pH to 7-8 to obtain thickened water, and add the thickened water in batches to the mixture obtained in step (2), maintain the temperature of the mixed system at 60-70° C., stir and emulsify, stop heating after the emulsion phase transition, add the remaining thickening water, continue stirring, and add the fungicide after the temperature of the mixed system drops to 35-40° C., mix evenly, and obtain a fermentation defoaming agent.

9. The method for preparing a fermentation defoamer according to claim 8, characterized in that: In step (3), the stirring speed of the stirring emulsification is 180 to 300 rpm.

Citation Information

Patent Citations

  • Emulsion-type organosilicone defoamer and preparation method thereof

    CN105688452A

  • Defoaming agent for wastewater zero discharge process and preparation method thereof

    CN112744886A

  • High-temperature-resistant organic silicon emulsion type defoaming agent and preparation method thereof

    CN114618190A

  • Preparation method and application of efficient and low-toxicity defoaming agent for biological fermentation