High-entropy metal oxide for carbon dioxide hydrogenation and preparation method thereof
The fluorite-type structure of high-entropy metal oxide catalyst and solution combustion method are prepared, and the problems of poor stability of existing catalysts under high temperature and high pressure conditions and difficult to improve reaction performance are solved, and carbon dioxide with high selectivity and thermal stability are achieved Hydrogenation to produce methanol reaction.
Patent Information
- Application Number
- CN202410999826.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-24
AI Technical Summary
The existing carbon dioxide hydrogenation methanol catalysts have poor stability under high temperature and high pressure conditions, and the reaction performance of composite metal oxide catalysts is difficult to improve, mainly due to the difficulty in adjusting the proportion of metal atoms and the problem of competitive adsorption of by-products.
A high-entropy metal oxide catalyst is used, which specifically constitutes a fluorite-type structure of CeO2, CuO, ZnO, Ga2O3 and ZrO2. It is prepared by solution combustion method to adjust the element ratio and structure to improve the selectivity and stability of the catalyst.
A high entropy metal oxide catalyst with excellent specific surface area, porous structure and thermal stability was achieved, which significantly improved the selectivity and yield of carbon dioxide hydrogenation to methanol, and its stability exceeded that of traditional Cu/ZnO/Al2O3 catalysts.
Smart Images

Figure CN118925734A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of high entropy oxide materials, and in particular relates to a high entropy metal oxide for carbon dioxide hydrogenation and a preparation method thereof. Background Art
[0002] As the problem of global warming becomes increasingly serious, the reduction and resource utilization of carbon dioxide have become key issues. Carbon dioxide is not only a major greenhouse gas, but is also often discharged as waste gas in industrial production. Therefore, finding an effective way to convert carbon dioxide into useful chemicals has become an important way to achieve carbon emission reduction goals. Carbon dioxide hydrogenation to methanol (CO2+3H2→CH3OH+H2O) is an effective carbon recycling technology. Through this reaction, carbon dioxide can be converted into an important chemical raw material-methanol. As a basic chemical raw material, methanol is widely used in fuels, solvents, plastics and pharmaceuticals. The optimization of its production process not only helps to improve resource utilization efficiency, but also reduces carbon dioxide emissions. The catalyst for the hydrogenation of carbon dioxide to methanol plays a vital role in this process. The performance of the catalyst directly affects the conversion rate and selectivity of the reaction, so the development of efficient and stable catalysts is the key to achieving industrial production.
[0003] At present, CO2 hydrogenation to methanol catalysts can be roughly divided into the following categories: transition metal catalysts, precious metal catalysts, and composite metal oxide catalysts, mainly copper-based catalysts. Among them, copper-based catalysts are the most widely used, which is attributed to the high reaction activity and methanol space-time yield of copper-based catalysts. However, the most widely studied Cu / ZnO / Al2O3 catalyst has poor water resistance, which makes the active site easy to sinter, seriously affecting its catalytic activity and stability. After a period of reaction, the activity begins to decline (patent publication number CN116020467A). Pt / In2O3 catalysts have anti-sintering, anti-poisoning and high stability, and have attracted widespread attention, but due to their high cost, they are not suitable for all-scale production (patent publication number CN118179498A). In recent years, composite metal oxide catalysts have shown excellent performance in CO2 hydrogenation to methanol. By regulating the composition and proportion of metal atoms in the composite metal oxide, the surface oxygen vacancy concentration can be increased and the reaction activity can be improved. For example, ZnZrO xThe Zn / (Zn+Zr) molar ratio in the system is 13%, and the reaction activity is optimal (Patent Publication No. CN116078370A), while the reaction activity decreases when the optimal ratio is exceeded. Therefore, from a macroscopic point of view, the phase change of the composite metal oxide caused by the increase in the proportion of metal atoms is the key to the difficulty in improving the reaction performance. In addition, the active sites of the binary composite metal oxide are not abundant enough, and there is competitive adsorption between CO2 and the reaction byproduct CO, especially the large amount of CO2 adsorption makes CO adsorption and hydrogenation difficult, which ultimately leads to a high selectivity of the byproduct CO.
[0004] High entropy metal oxides (HEMO) are single-phase stable solid solutions synthesized from five or more (nearly) equal molar ratio oxides, and their configurational entropy is greater than or equal to 1.5R ( R is the ideal gas constant, x i is the molar fraction of cations). Common single-phase high-entropy metal oxides currently formed include rock salt type, perovskite type, fluorite type, spinel type, etc. The unique properties of HEMO are very likely to solve the problems existing in ordinary composite metal oxides. (1) The multi-element characteristics of high-entropy metal oxides enable them to adjust the selectivity of catalytic reactions. By adjusting the ratio of different elements, the electronic structure of the catalyst can be optimized, thereby improving the selectivity for methanol production and reducing the occurrence of side reactions. (2) Due to the lattice distortion effect, a large number of oxygen vacancies can be generated on the surface of HEMO, promoting the activation of CO2 and H2. In addition, experimental reports have shown that the concentration of surface oxygen vacancies can be further increased by adding rare earth metal components to HEMO. (3) Due to the hysteresis diffusion effect, HEMO has high chemical stability, thermodynamic stability and mechanical stability, and can maintain good catalytic performance for a long time under complex and harsh conditions such as high temperature and high pressure.
[0005] However, the difficulty in preparing high-entropy metal oxide catalysts suitable for hydrogenation of carbon dioxide to methanol is mainly reflected in the following aspects: (1) The complexity of material design. High-entropy metal oxide catalysts usually contain multiple metal elements. The ratio, distribution and interaction of these elements have a significant impact on the performance of the catalyst. Designing such catalysts requires precise control of components and structures to achieve optimal catalytic activity and stability; (2) The challenge of synthesis methods. The synthesis of high-entropy metal oxide catalysts may require special high temperature, high pressure or atmosphere conditions, which may be difficult to control and may affect the microstructure and surface properties of the catalyst. In addition, the uniformity and purity during the synthesis process are also one of the challenges; (3) Optimization of catalytic performance. Even if a high-entropy metal oxide catalyst is successfully synthesized, ensuring that it has high activity, high selectivity and high stability is also a complex project. This requires fine control of the catalyst's surface chemistry, acidic center, electronic structure, etc. Summary of the invention
[0006] In order to solve the problems existing in the prior art, the purpose of the present invention is to provide a high entropy metal oxide for carbon dioxide hydrogenation and a preparation method thereof. The high entropy metal oxide of the present invention has the characteristics of high specific surface area, porous structure and excellent thermal stability.
[0007] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0008] A high entropy metal oxide for carbon dioxide hydrogenation, comprising components of CeO2, CuO, ZnO, Ga2O3 and ZrO2, wherein the molar ratio of the elements Ce, Cu, Zn, Ga and Zr is (3.9-4.1):(0.9-1.1):(0.9-1.1):(0.9-1.1):(0.9-1.1).
[0009] The method for preparing the high entropy metal oxide for carbon dioxide hydrogenation of the present invention comprises the following steps:
[0010] The complexing agent, the fuel and the metal salt containing the elements Ce, Cu, Zn, Ga and Zr are configured into a uniform mixed solution;
[0011] Evaporating excess water in the mixed solution until the mixed solution turns into a gel to obtain a gel-like substance;
[0012] causing the gel-like substance to undergo a combustion reaction in an air atmosphere to obtain a combustion product;
[0013] The combustion product is calcined in an air atmosphere, and after the calcination, the high entropy metal oxide for carbon dioxide hydrogenation is obtained.
[0014] Preferably, the metal salt comprises a rare earth metal salt or a transition metal salt corresponding to at least one element.
[0015] Preferably, the metal salt comprises one or more of nitrate, hydrochloride and acetate corresponding to at least one element.
[0016] Preferably, the fuel is any one or a mixture of glycine, urea, and glucose;
[0017] When the metal salt adopts the nitrate corresponding to the element, the ratio of the amount of substance of the fuel to the amount of substance of all element nitrates is 0.9-1.1.
[0018] Preferably, the complexing agent comprises citric acid and / or polyvinyl pyrrolidone, wherein the amount of the complexing agent is n1, the sum of the amounts of Ce, Cu, Zn, Ga and Zr is n2, and the ratio of n2:n1 is 0-0.5.
[0019] Preferably, when evaporating excess water in the mixed solution, the mixed solution is continuously stirred at 75-85° C. until the mixed solution turns into a gel state.
[0020] Preferably, when the gel-like substance is subjected to combustion reaction in an air atmosphere, the heating temperature is 295-305°C.
[0021] Preferably, when the combustion product is calcined in an air atmosphere, the calcination temperature is 395-405° C., the insulation time is 4.5-5.5 h, and the insulation is terminated after the calcination until the material is completely reacted, followed by natural cooling to obtain the high entropy metal oxide for carbon dioxide hydrogenation.
[0022] The use of the high entropy metal oxide for carbon dioxide hydrogenation of the present invention as described above, the high entropy metal oxide for carbon dioxide hydrogenation is used as a catalyst in the reaction of carbon dioxide hydrogenation to methanol, and the conditions for the reaction of carbon dioxide hydrogenation to methanol using the catalyst include:
[0023] The molar ratio of H2 to CO2 is 2 to 4;
[0024] The mass space velocity of the reaction is 2000-20000 mL / g cat h;
[0025] The reaction temperature is 280-350°C;
[0026] The reaction pressure is 3-5 MPa.
[0027] The present invention has the following beneficial effects:
[0028] The high entropy metal oxide for carbon dioxide hydrogenation of the present invention is a fluorite-type high entropy metal oxide based on cerium dioxide, and its components include: CeO2, CuO, ZnO, Ga2O3 and ZrO2, wherein CeO2 is a base material, which provides a stable oxide structure on the one hand, and on the other hand, the introduction of cerium is conducive to the generation of oxygen vacancies, and enhances the rare earth metal components of surface alkalinity to strengthen the activation of CO2 and H2; CuO can effectively promote the adsorption and activation of hydrogen and enhance the reaction activity of the catalyst; ZnO has the functions of support and electronic auxiliary agent, helps to adsorb H2, improve the dispersion of copper, and expose a larger specific surface area; Ga2O3 can dissociate H2 at high temperature, and within a certain temperature range, the higher the temperature, the stronger the dissociation ability of H2. In the reaction of methanol synthesis, Ga is mainly used as an auxiliary agent to improve the dispersion of active components Cu species and Zn species and improve the hydrogenation ability; ZrO2 is mainly responsible for the adsorption of CO2. The microstructure of the high entropy metal oxide used for carbon dioxide hydrogenation of the present invention is tested to be a porous structure with a high specific surface area. The experiment shows that the high entropy metal oxide has excellent thermal stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 Ce1 (CuZnGaZr) prepared in Example 1 and Example 2 of the present invention 1 / 4 XRD pattern of O4 fluorite high entropy metal oxide powder;
[0030] Figure 2 Ce1 (CuZnGaZr) prepared in Example 1 of the present invention 1 / 4 SEM image of O4 fluorite high entropy metal oxide powder;
[0031] Figure 3 Ce1 (CuZnGaZr) prepared in Example 2 of the present invention 1 / 4 SEM image of O4 fluorite-type high entropy metal oxide powder. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical solution and beneficial technical effect of the present invention clearer, the present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods. It should be understood that the specific implementation methods described in this specification are only for explaining the present invention, not for limiting the present invention.
[0033] The present invention is to prepare a fluorite-type high-entropy metal oxide (i.e., a high-entropy metal oxide for carbon dioxide hydrogenation of the present invention) by controlling the ratio of a complexing agent and a fuel using a solution combustion method, and the preparation method comprises the following steps:
[0034] (1) mixing a metal salt containing at least five metal elements, a complexing agent and a fuel to obtain a uniform mixed solution;
[0035] (2) stirring the mixed solution of step (1) to ensure that the metal ions, the complexing agent and the fuel are fully mixed;
[0036] (3) placing the mixed solution after stirring in step (2) on a heating plate and stirring, and evaporating excess water in the mixed solution at 80±5° C. until the mixed solution turns into a gel to obtain a gel-like substance;
[0037] (4) continuing to raise the temperature to 300±5° C. to allow the gel-like substance obtained in step (3) to undergo a combustion reaction in an air atmosphere. After the reaction is completed, the heating plate is turned off, and the combustion reaction product obtained is a fluffy black powder;
[0038] (5) The black powder obtained by the combustion reaction is transferred to a muffle furnace and calcined in an air atmosphere to finally obtain the high entropy metal oxide for carbon dioxide hydrogenation of the present invention.
[0039] Taking metal salts of five metal elements, namely Ce, Cu, Zn, Ga and Zr, as an example, the high entropy metal oxide for carbon dioxide hydrogenation obtained by the above method of the present invention is a fluorite-type high entropy metal oxide based on cerium dioxide, and its components include: CeO2, CuO, ZnO, Ga2O3 and ZrO2, wherein the molar ratio of the elements is Ce:Cu:Zn:Ga:Zr=(4±0.1):(1±0.1):(1±0.1):(1±0.1):(1±0.1).
[0040] In the above embodiment of the present invention, the metal salt includes a rare earth metal salt or a transition metal salt, and the metal salt may be one or more of nitrate, hydrochloride and acetate;
[0041] The complexing agent includes citric acid and / or polyvinyl pyrrolidone, preferably citric acid (CA). The complexing agent is a compound that can promote the dissolution of the precursor and stabilize the reaction process. Its functions include: a. Promoting dissolution. The complexing agent can react with metal ions (M n+ ) form complexes, enhancing the metal ion (M n+ )’s solubility in the solution helps to form a uniform solution. b. Control the reaction rate. The complexing agent can adjust the reaction rate and temperature, making the reaction process more controllable and avoiding too fast or too slow reaction speeds. c. Affect the properties of the catalyst. The choice of complexing agent can affect the structure, morphology and crystal structure of the final catalyst and adjust the properties of the catalyst. The amount of complexing agent citric acid is beneficial to the complexing of metal ions, but an increase in the amount of citric acid will increase the amount of oxidant required for the complete reaction; in the above-mentioned preparation method of the present invention, preferably, n(CA):n(M n+ )=0-0.5.
[0042] The fuel is any one or a combination of glycine, urea, and glucose, preferably glycine; the fuel releases a large amount of heat energy during combustion, providing the heat required for the reaction, promoting the decomposition of the precursor and the reaction. The combustion of the fuel also produces gases, such as carbon dioxide and water vapor, which help to form a uniform reaction environment and promote the dispersion of the precursor. The amount of fuel used and the ratio of nitrate will affect the properties of the prepared catalyst. The chemical reactions involved are as follows:
[0043]
[0044] M is a metal element; ν is the valence of the metal cation; is the molar ratio of fuel to oxidant, They correspond to the combustion conditions of lean combustion, rich combustion and chemical equivalent respectively. Generally, Preferred is 1-1.1.
[0045] The heating temperature of the combustion reaction in the above step (4) of the present invention is 300±5°C. The initial combustion reaction is usually carried out at a relatively high temperature, generating a high-temperature, high-speed flame and a violent combustion reaction. The heat released in this process can effectively convert the precursor into a metal oxide, and the powder produced in the combustion process is usually relatively fine and suitable for further processing.
[0046] The calcination temperature of the above step (5) of the present invention is 400±5°C, and the heating rate is 3°C / min. After calcination until the product is completely reacted, the insulation is terminated, and then naturally cooled. According to the test, under the experimental conditions of the present invention, the calcination time is 5 hours, which can ensure that the material is completely reacted. At this time, the insulation can be terminated. The specific calcination insulation time is related to the amount of raw materials used. Those skilled in the art can determine it according to actual conditions, and the present invention does not make specific limitations. Calcination helps to promote the crystallization of materials, remove impurities, enhance structural stability and improve performance. The calcination duration of step (5) is 4.5-5.5h.
[0047] In the above scheme of the present invention, since the weighing and heating equipment themselves have certain measurement errors, the data after the above "±" are all reasonable errors of the corresponding parameters. It can be foreseen that the technical scheme of the present invention is feasible within the above reasonable error range.
[0048] In the above step (1) of the present invention, the metal nitrate can be first accurately weighed according to the stoichiometric ratio, then dissolved in a certain amount of distilled water, and stirred evenly at room temperature to obtain a mixed solution of five metal cations.
[0049] The use of the high entropy metal oxide for carbon dioxide hydrogenation of the present invention as a catalyst: The reaction of carbon dioxide hydrogenation to methanol is a reaction in which the number of molecules is reduced. The efficient activation of CO2 requires high temperature to overcome the kinetic barrier. Therefore, in order to increase the methanol yield, the reaction needs to be carried out at high temperature and high pressure, as follows:
[0050] The molar ratio of H2 to CO2 is 2 to 4;
[0051] The mass space velocity of the reaction is 2000-20000 mL / g cat h;
[0052] The reaction temperature is 280-350°C;
[0053] The reaction was carried out in a fixed bed reactor, the reaction tube had an inner diameter of 8 mm and a length of 300 mm;
[0054] The reaction pressure is 3-5 MPa.
[0055] The following embodiments of the present invention are to prepare metal nitrate according to the chemical formula Ce1(CuZnGaZr): 1 / 4The stoichiometric ratio of O4 is accurately weighed, dissolved in a certain amount of distilled water, and stirred evenly at room temperature to obtain a mixed solution of five metal cations.
[0056] Example 1
[0057] In this embodiment, a solution combustion method is used to prepare a high entropy metal oxide for carbon dioxide hydrogenation, and its chemical formula is Ce1(CuZnGaZr): 1 / 4 O4.
[0058] The preparation method of the high entropy metal oxide for carbon dioxide hydrogenation in this embodiment comprises the following steps:
[0059] (1) accurately weighing the corresponding metal nitrates according to the stoichiometric ratio of the molecular formula, specifically 4.343 g of Ce(NO3)3·6H2O, 0.610 g of Cu(NO3)2·3H2O, 0.751 g of Zn(NO3)2·6H2O, 0.639 g of Ga(NO3)3 and 1.073 g of Zr(NO3)4·5H2O, then dissolving all the nitrates in 300 mL of distilled water, and stirring evenly at room temperature to obtain a mixed solution containing five metal cations;
[0060] (2) Then according to n(CA):n(M n+ )=0, i.e. no citric acid is added; Add 2.398g of glycine in a ratio of 1.5 and stir evenly to mix the metal ions and fuel in the solution evenly;
[0061] (3) placing the mixed solution on a heating plate and stirring, evaporating excess water from the mixed solution at 80±5°C, and drying the mixed solution until it becomes a gel;
[0062] (4) Continue to raise the temperature to 300±5°C to allow the mixed liquid to undergo a combustion reaction in an air atmosphere. After the reaction is completed, turn off the heating plate to obtain a fluffy black powder;
[0063] (5) The obtained powder was transferred to a muffle furnace for calcination at a temperature of 400±5°C, a heating rate of 3°C / min, and a holding time of 5 h. After the calcination, the powder was naturally cooled to finally obtain a high entropy metal oxide sample.
[0064] Depend on Figure 1 It can be seen that the diffraction peak intensity of the sample synthesized with glycine as fuel without adding citric acid is higher and the peak shape is sharp, indicating that the crystallinity of the powder is higher. Figure 2 It can be seen that the powders prepared by the solution combustion method all have a porous network structure. This is mainly caused by the instantaneous release of a large amount of gas by nitrates and fuels during the combustion process. This phenomenon is conducive to increasing the specific surface area of the material, thereby improving the reaction activity.
[0065] The experiment of producing methanol by hydrogenation of CO2 catalyzed by high entropy metal oxides was carried out in a fixed bed reactor under certain conditions such as temperature, pressure, space velocity and CO2 / H2 feed ratio. The product distribution was analyzed by gas chromatography. The activity and selectivity of the CO2 hydrogenation to methanol reaction catalyzed by high entropy metal oxides under different reaction conditions were investigated. The catalyst performance was evaluated based on indicators such as CO2 conversion rate, methanol selectivity, yield and catalyst stability. The details are as follows:
[0066] The performance evaluation of high entropy metal oxide catalysts was carried out in a continuous flow fixed bed reactor. 0.2 g of catalyst diluted with quartz sand (all 60-80 mesh) was loaded into a stainless steel tubular reactor. Before the catalytic measurement, the fresh catalyst was reduced in a 10 vol% H2 / N2 gas flow at 300±5℃ for 3 hours at normal pressure. Then, the reactor was cooled to 200±5℃, the reaction gas (CO2:H2=1:3, molar) was introduced, the pressure was raised to 3.0MPa, and the temperature was raised to 300±5℃. All pipelines and valves after the reactor were heated to 150±5℃ to prevent product condensation. Four hours after the start of the reaction, the effluent products were analyzed online using a gas chromatograph to calculate the carbon dioxide conversion rate and methanol selectivity. Under this condition, the CO2 conversion rate reached 10.7%, the methanol selectivity reached 72%, and it was stable for more than 30h, which was better than Cu / ZnO / Al2O3 in selectivity and thermal stability. The specific results are shown in Table 1.
[0067] Example 2
[0068] The preparation method of the high entropy metal oxide for carbon dioxide hydrogenation in this embodiment comprises the following steps:
[0069] (1) The second fluorite-type high entropy oxide catalyst of the present invention is prepared by solution combustion method, and its chemical formula is Ce1(CuZnGaZr): 1 / 4 O4. Accurately weigh the corresponding metal nitrates according to the stoichiometric ratio of the molecular formula, specifically 4.343g of Ce(NO3)3·6H2O, 0.610g of Cu(NO3)2·3H2O, 0.751g of Zn(NO3)2·6H2O, 0.639g of Ga(NO3)3 and 1.073g of Zr(NO3)4·5H2O, then dissolve all the nitrates in 300mL of distilled water, stir evenly at room temperature, and obtain a mixed solution containing five metal cations;
[0070] (2) Then according to n(CA):n(M n+ )=0.5, add 2.101g citric acid; according to Add 2.398g of glycine in a ratio of 1.5 and stir evenly to mix the metal ions and fuel in the solution evenly;
[0071] (3) placing the mixed solution on a heating plate and stirring, evaporating excess water from the mixed solution at 80±5°C, and drying the mixed solution until it becomes a gel;
[0072] (4) Continue to raise the temperature to 300±5°C to allow the mixed liquid to undergo a combustion reaction in an air atmosphere. After the reaction is completed, turn off the heating plate to obtain a fluffy black powder;
[0073] (5) The obtained powder was transferred to a muffle furnace for calcination at a temperature of 400±5°C, a heating rate of 3°C / min, and a holding time of 5 h. After the calcination, the powder was naturally cooled to finally obtain a high entropy metal oxide sample.
[0074] from Figure 1 It can be seen that the characteristic peaks of the powders obtained in Example 1 and Example 2 are completely consistent, indicating that the crystal structure of the powders has not changed after the addition of citric acid. However, the XRD spectrum of the sample with citric acid added has a slightly weaker characteristic diffraction peak intensity and a wider peak width. According to the Scherrer formula, it can be estimated that the sample has smaller crystals and a larger specific surface area, which is more conducive to improving the reaction activity. This result can also be compared with Figure 2 , Figure 3 The SEM images of the samples corroborate each other.
[0075] The catalyst performance evaluation procedure is the same as in Example 1, as shown in Table 1.
[0076] Table 1
[0077]
[0078] Reaction conditions: n(H2):n(CO2)=3:1, 3MPa, 300±5℃, 8000mL·g -1 ·h -1
[0079] It can be seen that the high-entropy metal oxide catalyst prepared by adding an appropriate amount of citric acid performs better, the conversion rate of carbon dioxide and the yield of product methanol are both improved, and no deactivation occurs after 30 hours of reaction.
[0080] In summary, the present invention brings the following beneficial technical effects:
[0081] The present invention uses a solution combustion method to prepare a high entropy metal oxide catalyst suitable for hydrogenation of carbon dioxide to methanol. Its advanced features are reflected in the following aspects:
[0082] (1) High entropy metal oxides have high thermal stability, which enables them to maintain good catalytic activity at high temperatures. For CO2 hydrogenation reactions that need to be carried out at high temperatures, no deactivation occurs after 30 hours of continuous reaction;
[0083] (2) Compared with the commercial catalyst Cu / ZnO / Al2O3, the selectivity and yield of the product methanol were significantly improved when high entropy metal oxides were used for hydrogenation of carbon dioxide to produce methanol.
[0084] (3) The solution combustion method for preparing high entropy metal oxides has the advantages of simple operation, using mostly transition metal salts as raw materials, low cost, and high product uniformity;
[0085] (4) The most widely used catalyst for the hydrogenation of CO2 to methanol in industry is a copper-based catalyst (such as Cu / ZnO / Al2O3), which has the characteristics of high reactivity, but poor water resistance, easy sintering of active sites, and poor stability. The present invention can obtain a high-entropy metal oxide catalyst with high specific surface area, porous structure, and excellent thermal stability, which can be applied to the hydrogenation of carbon dioxide to methanol reaction.
[0086] In summary, the catalyst prepared by the present invention exhibits efficient and stable catalytic performance, has a low preparation cost, and the preparation method has good universality, showing good application prospects in the field of carbon dioxide resource utilization.
[0087] The technical solution provided by the present invention demonstrates its unique principles and application potential through the above-mentioned embodiments. However, the present invention is not limited to the embodiments described, but covers any specific methods, material preparations and conclusions that conform to its technical essence. Any reasonable changes to the existing embodiments, or equivalent modifications based on the principles of the present invention, should not exceed the scope of protection of the present invention.
[0088] Therefore, the present invention welcomes academic exploration and technical practice from all aspects, aiming to promote scientific and technological progress and innovative development in related fields. Any interested individual or organization can further carry out in-depth research and application development based on the technical solution of the present invention, and jointly contribute to the progress of science and technology.
Claims
1. A high entropy metal oxide for carbon dioxide hydrogenation, characterized in that: Its components include: CeO2, CuO, ZnO, Ga2O3 and ZrO2, wherein the molar ratio of the elements Ce, Cu, Zn, Ga and Zr is (3.9-4.1):(0.9-1.1):(0.9-1.1):(0.9-1.1):(0.9-1.1).
2. The method for preparing the high entropy metal oxide for carbon dioxide hydrogenation according to claim 1, characterized in that: The process includes the following: The complexing agent, the fuel and the metal salt containing the elements Ce, Cu, Zn, Ga and Zr are configured into a uniform mixed solution; Evaporating excess water in the mixed solution until the mixed solution turns into a gel to obtain a gel-like substance; causing the gel-like substance to undergo a combustion reaction in an air atmosphere to obtain a combustion product; The combustion product is calcined in an air atmosphere, and after the calcination, the high entropy metal oxide for carbon dioxide hydrogenation is obtained.
3. The method for preparing a high entropy metal oxide for carbon dioxide hydrogenation according to claim 2, characterized in that: The metal salt comprises a rare earth metal salt or a transition metal salt corresponding to at least one element.
4. The method for preparing a high entropy metal oxide for carbon dioxide hydrogenation according to claim 2, characterized in that: The metal salt includes one or more of nitrate, hydrochloride and acetate corresponding to at least one element.
5. The method for preparing a high entropy metal oxide for carbon dioxide hydrogenation according to claim 4, characterized in that: The fuel is any one of glycine, urea and glucose or a mixture of several of them; When the metal salt adopts the nitrate corresponding to the element, the ratio of the amount of substance of the fuel to the amount of substance of all element nitrates is 0.9-1.
1.
6. The method for preparing a high entropy metal oxide for carbon dioxide hydrogenation according to claim 2, characterized in that: The complexing agent comprises citric acid and / or polyvinyl pyrrolidone, wherein the amount of the complexing agent is n1, the sum of the amounts of Ce, Cu, Zn, Ga and Zr is n2, and the ratio of n2:n1 is 0-0.
5.
7. The method for preparing a high entropy metal oxide for carbon dioxide hydrogenation according to claim 2, characterized in that: When the excess water in the mixed solution is evaporated, the mixed solution is continuously stirred at 75-85° C. until the mixed solution turns into a gel state.
8. The method for preparing a high entropy metal oxide for carbon dioxide hydrogenation according to claim 2, characterized in that: When the gel-like substance is subjected to combustion reaction in an air atmosphere, the heating temperature is 295-305°C.
9. The method for preparing a high entropy metal oxide for carbon dioxide hydrogenation according to claim 2, characterized in that: When the combustion product is calcined in an air atmosphere, the calcination temperature is 395-405° C. After the calcination is completed, the heat preservation is terminated, and then the product is naturally cooled to obtain the high entropy metal oxide for carbon dioxide hydrogenation.
10. The use of the high entropy metal oxide for carbon dioxide hydrogenation according to claim 1, characterized in that: The high entropy metal oxide for hydrogenation of carbon dioxide is used as a catalyst for the reaction of hydrogenation of carbon dioxide to methanol. The conditions for the reaction of hydrogenation of carbon dioxide to methanol using the catalyst include: The molar ratio of H2 to CO2 is 2 to 4; The mass space velocity of the reaction is 2000-20000 mL / g cat h; The reaction temperature is 280-350°C; The reaction pressure is 3-5 MPa.
Citation Information
Patent Citations
Segmented roasting method of Cu / ZnO / Al2O3 catalyst
CN116020467A
Catalyst for preparing methanol through carbon dioxide hydrogenation and preparation and application thereof
CN116078370A
Monatomic Pt-doped indium oxide catalyst as well as preparation method and application thereof
CN118179498A
Catalyst for preparing methanol by carbon dioxide hydrogenation and preparation method thereof
CN106902833A
Catalyst for preparing methanol through hydrogenation of carbon dioxide and preparation method thereof