Copper-nickel composite catalytic material as well as preparation method and application thereof
Through the combination of copper-nickel composite catalytic material and persulfate, high-reactive free radicals are generated, which solves the problems of low degradation efficiency of antibiotic contaminated water and limited pH range in the prior art, and achieves efficient removal of antibiotics and Environmentally friendly water treatment.
Patent Information
- Application Number
- CN202411404208.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-10
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-10-10
AI Technical Summary
Prior Art When treating antibiotic contaminated water, advanced oxidation technologies (AOPs) have low degradation efficiency for antibiotics and have limited pH range, so they cannot effectively remove antibiotic contaminants in water.
The copper-nickel composite catalytic material (Cu2O(SO4)/NiO) was prepared by hydrothermal synthesis and calcination as a heterogeneous catalyst, combined with hydropersulfate (PMS) activation, to generate highly active free radicals to degrade antibiotics.
It significantly improves the degradation efficiency of antibiotics and is suitable for wastewater with a pH range of 3 to 11. The degradation effect is better than that of Cu2O or NiO catalytic materials alone. The material is stable and has low cost, avoiding secondary pollution.
Smart Images

Figure CN118925755A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water pollution treatment, and in particular relates to a copper-nickel composite catalytic material and a preparation method and application thereof. Background Art
[0002] In recent years, the presence of antibiotics in the environment has attracted great attention due to their toxic effects on aquatic species and bacterial resistance, even at low concentrations. These compounds reach the aquatic environment through various sources, such as pharmaceutical factories, hospital wastewater, domestic wastewater, and through human and livestock discharge. With the increasing awareness of the relationship between man and the environment, the call for environmental protection is getting louder. The problem of water pollution not only restricts economic development, but also endangers human health and even social stability. Therefore, the treatment of antibiotic wastewater is of great significance for environmental remediation. Compared with traditional wastewater treatment technologies such as biodegradation and physical adsorption, advanced oxidation technology (AOPs) has attracted widespread attention by producing free radicals with low selectivity and high reactivity to oxidatively degrade antibiotics.
[0003] Advanced oxidation process is a kind of process that produces highly active oxidants (such as •OH, SO4• - ) is a method for degrading organic pollutants. Sulfate radical-based AOPs (SR-AOPs) have attracted more and more attention in the field of water treatment due to their high efficiency, economy and environmental friendliness. Persulfate (PMS) is a commonly used activator. It activates PMS to produce sulfate radicals (SO4• - ) mainly produce active oxygen free radicals, which oxidize organic pollutants into CO2, H2O and harmless or less harmful chemicals. Summary of the invention
[0004] In order to overcome the shortcomings and deficiencies of the prior art, the object of the present invention is to provide a copper-nickel composite catalytic material and a preparation method and application thereof.
[0005] The present invention is achieved by a method for preparing a copper-nickel composite catalytic material, the method comprising the following steps: (1) Dissolve 1-3 mmol of Ni(NO3)2•6H2O and 3-5 mmol of Cu(NO3)2•3H2O in a mixed solution of 25 mL of deionized water and 25 mL of ethylene glycol to obtain solution A; 24 mmol of thiourea was dissolved in a mixed solution of 10 mL of deionized water and 10 mL of ethylene glycol to obtain solution B; Solution B was added dropwise into solution A, and after vigorous stirring, the mixture was transferred into a high-pressure reactor for hydrothermal reaction, and a precursor was obtained after the reaction was completed; (2) Washing and drying the obtained precursor, calcining and grinding the dried precursor to obtain a Cu2O(SO4) / NiO composite catalytic material.
[0006] Preferably, in step (1), 2 mmol of Ni(NO3)2•6H2O and 4 mmol of Cu(NO3)2•3H2O are dissolved in a mixed solution of 25 mL of deionized water and 25 mL of ethylene glycol to obtain solution A.
[0007] Preferably, in step (1), the temperature of the hydrothermal reaction is 160-200° C. and the time is 20-28 h.
[0008] Preferably, in step (2), the calcination temperature is 500-800°C, the heating rate is 5°C / min, and the calcination time is 1-4 h.
[0009] The invention further discloses a copper-nickel composite catalytic material prepared by the method.
[0010] The invention further discloses the application of the copper-nickel composite catalytic material in activating persulfate to degrade antibiotic pollutants in wastewater.
[0011] Preferably, the antibiotic pollutants include ciprofloxacin, levofloxacin and tetracycline, and the pH value of the wastewater is 3-11.
[0012] The present invention overcomes the deficiencies of the prior art and provides a copper-nickel composite catalytic material and a preparation method and application thereof. The present invention successfully prepares a copper-nickel composite catalytic material (Cu2O (SO4) / NiO composite catalytic material) by hydrothermal synthesis and calcination. The transition metal in the composite catalytic material has the characteristics of multivalence, low toxicity and low cost, and Cu2O (SO4) is an oxygen-containing sulfate with rich chemical composition and a three-dimensional structure, which can effectively promote electron transfer, thereby generating more active species, which is beneficial to the degradation of organic pollutants. Therefore, the composite catalytic material, as a highly active heterogeneous catalyst, can be effectively applied to the degradation of organic pollutants.
[0013] Compared with the shortcomings and deficiencies of the prior art, the present invention has the following beneficial effects: (1) The composite catalytic material of the present invention has significant catalytic performance, and can effectively degrade antibiotics in wastewater by activating PMS. More active free radicals are generated by activating PMS to effectively degrade antibiotic pollutants such as ciprofloxacin, levofloxacin, and tetracycline; (2) The composite catalytic material of the present invention can degrade antibiotic wastewater with a wide pH value range, and the pH value range of antibiotic wastewater can reach 3~11; compared with single Cu2O (SO4), NiO, etc., the composite catalytic material has a better ability to activate PMS to degrade antibiotics; (3) The composite catalytic material of the present invention has good removal effect on antibiotics in wastewater, is clean and pollution-free, and is a catalytic material that can be widely used and can efficiently remove antibiotics in water bodies; and the Cu2O(SO4) / NiO catalytic material has good stability, a simple and easy-to-operate preparation process, low cost, and the degradation process does not cause secondary pollution to the environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 It is the XRD diffraction pattern of the Cu2O (SO4) catalytic material, the NiO catalytic material, and the Cu2O (SO4) / NiO (4:2) composite catalytic material in the embodiment of the present invention; Figure 2 The SEM and TEM images of the Cu2O (SO4) catalytic material, the NiO catalytic material, and the Cu2O (SO4) / NiO (4:2) composite catalytic material in the embodiment of the present invention are shown; wherein, Figure 2 a is the SEM image of Cu2O (SO4) catalytic material, Figure 2 b is the SEM image of NiO catalytic material. Figure 2 c is the SEM image of Cu2O (SO4) / NiO (4:2) catalytic material, Figure 2 d is the TEM image of Cu2O(SO4) / NiO (4:2) catalytic material; Figure 3 It is a comparison chart of the degradation efficiency of Cu2O (SO4) catalytic material, NiO catalytic material, and Cu2O (SO4) / NiO (4:2) composite catalytic material on ciprofloxacin (CIP) in the effect embodiment of the present invention; Figure 4 This is a comparison chart of the degradation efficiency of ciprofloxacin (CIP) by three groups of composite catalytic materials with different molar ratios of Cu2O (SO4) and NiO in the effect embodiment of the present invention; Figure 5 It is a comparison chart of the degradation efficiency of ciprofloxacin (CIP) of the Cu2O (SO4) / NiO (4:2) composite catalytic material at different dosages and different dosages of persulfate in the effect embodiment of the present invention; wherein, Figure 5 a is the degradation efficiency diagram of ciprofloxacin (CIP) at different dosages of Cu2O (SO4) / NiO (4:2) composite catalytic material. Figure 5 b is the degradation efficiency diagram of ciprofloxacin (CIP) at different dosages of PMS; Figure 6This is a graph showing the degradation of ciprofloxacin (CIP) by the Cu2O (SO4) / NiO (4:2) composite catalytic material under the influence of different anions and humic acid in the embodiment of the present invention; wherein, Figure 6 a~c are anions Cl - 、NO3 - and HCO3 - Degradation diagram of ciprofloxacin (CIP) under the influence of Figure 6 d is the degradation diagram of ciprofloxacin (CIP) under the influence of humic acid (HA); Figure 7 This is a graph showing the degradation of ciprofloxacin (CIP) at different concentrations by the Cu2O (SO4) / NiO (4:2) composite catalytic material in an embodiment of the present invention. DETAILED DESCRIPTION
[0015] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. Example 1
[0016] 1. Preparation of Cu2O (SO4) catalytic materials (1) Dissolve 6 mmol of Cu(NO3)2•3H2O in a mixed solution of 25 mL of deionized water and 25 mL of ethylene glycol to obtain solution A, and stir on a magnetic stirrer for 20 min; 24 mmol of thiourea was dissolved in a mixed solution of 10 mL of deionized water and 10 mL of ethylene glycol to obtain solution B, which was stirred on a magnetic stirrer for 20 min; Solution B was added dropwise into solution A, and after vigorous stirring for 20 min, the mixture was transferred into a high-pressure reactor for hydrothermal reaction at 180 °C for 24 h. After the reaction, a precursor was obtained. (2) The obtained precursor was washed with deionized water and anhydrous ethanol three times respectively, and then placed in a drying oven for drying. The dried precursor was calcined for 2 h at a temperature of 700 °C and a heating rate of 5 °C / min to obtain a Cu2O (SO4) catalytic material.
[0017] 2. Preparation of NiO catalytic materials (1) Dissolve 6 mmol of Ni(NO3)2•6H2O in a mixed solution of 25 mL of deionized water and 25 mL of ethylene glycol to obtain solution A, and stir on a magnetic stirrer for 20 min; 24 mmol of thiourea was dissolved in a mixed solution of 10 mL of deionized water and 10 mL of ethylene glycol to obtain solution B, which was stirred on a magnetic stirrer for 20 min; Solution B was added dropwise into solution A, and after vigorous stirring for 20 min, the mixture was transferred into a high-pressure reactor for hydrothermal reaction at 180 °C for 24 h. After the reaction, a precursor was obtained. (2) The obtained precursor was washed with deionized water and anhydrous ethanol three times respectively, and then placed in a drying oven for drying. The dried precursor was calcined for 2 hours at a temperature of 700°C and a heating rate of 5°C / min to obtain a NiO catalytic material. Example 2
[0018] (1) Dissolve 2 mmol of Ni(NO3)2•6H2O and 4 mmol of Cu(NO3)2•3H2O in a mixed solution of 25 mL of deionized water and 25 mL of ethylene glycol to obtain solution A, and stir on a magnetic stirrer for 20 min; 24 mmol of thiourea was dissolved in a mixed solution of 10 mL of deionized water and 10 mL of ethylene glycol to obtain solution B, which was stirred on a magnetic stirrer for 20 min; Solution B was added dropwise into solution A, and after vigorous stirring for 20 min, the mixture was transferred into a high-pressure reactor for hydrothermal reaction at 180 °C for 24 h. After the reaction, a precursor was obtained. (2) The obtained precursor was washed with deionized water and anhydrous ethanol three times respectively, and then placed in a drying oven for drying (60°C). The dried precursor was calcined for 2 h at a temperature of 700°C and a heating rate of 5°C / min to obtain a composite catalytic material with a molar ratio of Cu2O (SO4) to NiO of 4:2, i.e., Cu2O (SO4) / NiO (4:2) composite catalytic material. Example 3
[0019] The preparation method of this embodiment is basically the same as that of Example 2, except that: Ni(NO3)2•6H2O is 1 mmol, Cu(NO3)2•3H2O is 5 mmol, and the molar ratio of Cu2O(SO4) and NiO in the obtained material is 5:1, i.e., Cu2O(SO4) / NiO (5:1) composite catalytic material. Example 4
[0020] The preparation method of this embodiment is basically the same as that of Example 2, except that: Ni(NO3)2•6H2O is 3 mmol, Cu(NO3)2•3H2O is 3 mmol, and a composite catalytic material with a molar ratio of Cu2O(SO4) to NiO of 3:3 is obtained, namely, Cu2O(SO4) / NiO (3:3) composite catalytic material. Example 5
[0021] (1) Dissolve 3 mmol of Ni(NO3)2•6H2O and 3 mmol of Cu(NO3)2•3H2O in a mixed solution of 25 mL of deionized water and 25 mL of ethylene glycol to obtain solution A, and stir on a magnetic stirrer for 20 min; 24 mmol of thiourea was dissolved in a mixed solution of 10 mL of deionized water and 10 mL of ethylene glycol to obtain solution B, which was stirred on a magnetic stirrer for 20 min; Solution B was added dropwise into solution A, and after vigorous stirring for 20 min, the mixture was transferred into a high-pressure reactor for hydrothermal reaction at 160 °C for 20 h. After the reaction, a precursor was obtained. (2) The obtained precursor was washed with deionized water and anhydrous ethanol three times respectively, and then placed in a drying oven for drying (60°C). The dried precursor was calcined for 1 h at a temperature of 500°C and a heating rate of 5°C / min to obtain a Cu2O(SO4) / NiO (3:3) composite catalytic material. Example 6
[0022] (1) Dissolve 2 mmol of Ni(NO3)2•6H2O and 4 mmol of Cu(NO3)2•3H2O in a mixed solution of 25 mL of deionized water and 25 mL of ethylene glycol to obtain solution A, and stir on a magnetic stirrer for 20 min; 24 mmol of thiourea was dissolved in a mixed solution of 10 mL of deionized water and 10 mL of ethylene glycol to obtain solution B, which was stirred on a magnetic stirrer for 20 min; Solution B was added dropwise into solution A, and after vigorous stirring for 20 min, the solution was transferred into a high-pressure reactor for hydrothermal reaction. The hydrothermal time was 28 h at a temperature of 200 °C. After the reaction, a precursor was obtained. (2) The obtained precursor was washed with deionized water and anhydrous ethanol three times respectively, and then placed in a drying oven for drying (60°C). The dried precursor was calcined for 4 hours at a temperature of 800°C and a heating rate of 5°C / min to obtain a Cu2O (SO4) / NiO (4:2) composite catalytic material.
[0023] Effect Example 1 The following tests were performed on the Cu2O (SO4) catalytic material, NiO catalytic material, and Cu2O (SO4) / NiO (4:2) composite catalytic material samples prepared in Examples 1-2.
[0024] 1. Sample test characterization XRD tests were performed on Cu2O (SO4) catalytic materials, NiO catalytic materials, and Cu2O (SO4) / NiO (4:2) composite catalytic materials. The obtained XRD diffraction patterns are as follows: Figure 1 As shown. Figure 1 It can be seen that the diffraction peaks corresponding to the Cu2O (SO4) / NiO (4:2) composite catalytic material sample correspond to the crystal planes of the Cu2O (SO4) catalytic material and the NiO catalytic material, respectively. Figure 2 SEM and TEM showed that spherical NiO was attached to the surface of Cu2O (SO4). From the above characterization, it can be seen that the Cu2O (SO4) / NiO (4:2) composite catalytic material was successfully prepared.
[0025] 2. Test on degradation of antibiotics in water Use a measuring cylinder to measure 100 mL of 10 mg / L ciprofloxacin solution into a conical flask. Perform the following 6 experiments at the same time, adding the following degradation materials: (1) No addition, blank group; (2) 30 mg persulfate (PMS); (3) 30 mg Cu2O(SO4) / NiO(4:2) composite catalytic material; (4) 30 mg Cu2O (SO4) catalytic material + 30 mg PMS; (5) 30 mg NiO catalytic material + 30 mg PMS; (6) 30 mg Cu2O (SO4) / NiO (4:2) composite catalytic material + 30 mg PMS.
[0026] Each experimental group was placed on a magnetic stirrer, the speed was adjusted to a certain level, and samples were taken at specific intervals. After sampling, the absorbance was measured using a UV-visible spectrophotometer. The results were as follows: Figure 3 As shown, the degradation rate of ciprofloxacin was calculated by absorbance, degradation rate = (1-C / C0) × 100%.
[0027] Depend on Figure 3It can be seen that the blank group and the experimental group with the addition of Cu2O (SO4) / NiO (4:2) composite catalytic material alone have almost no degradation effect on ciprofloxacin. The experimental group with only PMS added has a certain degradation of ciprofloxacin, but the degradation efficiency is very low. The experimental group with the addition of Cu2O (SO4) / NiO (4:2) composite catalytic material and PMS at the same time has a significantly improved degradation efficiency of ciprofloxacin. The degradation rate of ciprofloxacin can reach about 79.4% at 60 minutes of degradation, which has a good effect and good stability. The catalytic materials prepared in Example 1 have a certain degree of degradation of CIP, but the Cu2O (SO4) / NiO (4:2) composite catalytic material prepared in Example 2 has the strongest ability to degrade ciprofloxacin compared with the catalytic material prepared in Example 1. It can be seen that after adding PMS, the Cu2O (SO4) / NiO (4:2) composite catalytic material activates persulfate (PMS), which can promote the generation of active free radicals and improve the degradation efficiency of pollutants in water.
[0028] Effect Example 2 Three groups of degradation experiments were set up using the Cu2O(SO4) / NiO(4:2) composite catalytic material prepared in Example 2 and the Cu2O(SO4) / NiO(5:1) composite catalytic material and the Cu2O(SO4) / NiO(3:3) composite catalytic material prepared in Examples 3 to 4 as catalysts.
[0029] Three groups of water to be treated were placed in 100 mL conical flasks respectively. 30 mg of catalyst and 30 mg of PMS were added to each group of water to be treated. The conical flasks containing the water to be treated were placed on a magnetic stirrer. After a certain period of degradation, the water to be treated was filtered. The degradation results are shown in the figure. Figure 4 As shown. Figure 4 It can be seen that the Cu2O (SO4) / NiO / PMS system has a certain degree of degradation of CIP, among which the Cu2O (SO4) / NiO (4:2) composite catalytic material prepared in Example 2 activated PMS has stronger degradation ability for CIP than the catalytic degradation performance of the other two groups of composite catalytic materials.
[0030] Effect Example 3 An experimental analysis was conducted on the effects of the dosage of Cu2O (SO4) / NiO catalytic materials and PMS on the degradation effect during the degradation process.
[0031] 1. The effect of the dosage of the Cu2O (SO4) / NiO (4:2) composite catalytic material prepared in Example 2 on the degradation efficiency was experimentally studied. 30 mg, 40 mg, 50 mg, 60 mg, and 70 mg of the Cu2O (SO4) / NiO (4:2) composite catalytic material were used as catalysts, ciprofloxacin solution was used as the solution to be degraded, and 30 mg of PMS was added to carry out degradation experiments. After sampling, the absorbance was measured by a UV-visible spectrophotometer. The results are as follows: Figure 5 As shown in (a), it can be seen that the amount of Cu2O (SO4) / NiO (4:2) composite catalyst material has a certain influence on the degradation efficiency. The degradation efficiency is best when the amount of Cu2O (SO4) / NiO (4:2) composite catalyst material is 50 mg, so the catalyst is selected to continue the study. Cu2O (SO4) / NiO (4:2) composite catalyst material can catalyze PMS to produce SO4 with strong oxidizing properties. − and •OH react with pollutants and then degrade them into small molecules of CO2 and H2O.
[0032] 2. Using the Cu2O (SO4) / NiO (4:2) composite catalytic material prepared in Example 2 as a catalyst, 5 groups of degradation experiments with different addition amounts of PMS were set up. First, 5 groups of water to be treated were placed in 100 mL conical flasks, 50 mg of catalyst was added to each group of water to be treated, and 30 mg, 40 mg, 50 mg, 60 mg, and 70 mg of PMS were added at the same time. The conical flask containing the water to be treated was placed on a magnetic stirrer. After a certain period of degradation, the water to be treated was filtered. The degradation results are shown in the figure. Figure 5 (b) As shown in Figure 5 (b) It can be seen that when the catalyst dosage is 50 mg, the degradation rate of CIP in the system with a PMS dosage of 50 mg is the highest, reaching 90.0%.
[0033] Effect Example 4 The effects of coexisting anions and organic matter in the degradation wastewater on the Cu2O (SO4) / NiO catalytic material were tested.
[0034] Using the Cu2O(SO4) / NiO(4:2) composite catalytic material prepared in Example 2 as the catalyst, four groups of degradation experiments were set up. First, the four groups of water to be treated were placed in 100 mL conical flasks, 50 mg of degradation material was added to each group of water to be treated, and 50 mg of PMS was added at the same time. Cl was added to each of the four groups of experiments. - 、NO3 - 、HCO3 -and humic acid (HA). The addition amounts of the four substances were set to 5 mmol, 10 mmol, 15 mmol and 20 mmol respectively. The conical flask containing the water to be treated was placed on a magnetic stirrer. After degradation for a certain period of time, the water to be treated was filtered.
[0035] Degradation results such as Figure 6 As shown by Figure 6 It can be seen that Cl - HA has little effect on the degradation efficiency of PMS activated by catalyst for CIP degradation, while higher concentrations of HCO3 - and NO3 - It has a certain influence on the degradation ability of ciprofloxacin (CIP) antibiotics, which may be due to HCO3 - and NO3 - It is caused by the consumption or attachment of a certain amount of active substances.
[0036] Effect Example 5 The effect of Cu2O(SO4) / NiO catalytic material on the degradation of different concentrations of ciprofloxacin (CIP) was analyzed.
[0037] Using the Cu2O (SO4) / NiO (4:2) composite catalytic material prepared in Example 2 as a catalyst, four groups of degradation experiments were set up to analyze the degradation of different concentrations of ciprofloxacin by the catalytic material. First, different concentrations of ciprofloxacin were prepared. Ciprofloxacin solutions with concentrations of 5 mg / L, 10 mg / L, 15 mg / L, and 20 mg / L were placed in 100 mL conical flasks. 50 mg of catalyst and 50 mg of PMS were added to each group of treated water. The conical flask containing the water to be treated was placed on a magnetic stirrer. After a certain period of degradation, the water to be treated was filtered. Figure 7 It can be seen that the Cu2O (SO4) / NiO (4:2) composite catalytic material activated PMS also has a good degradation effect on high concentration of ciprofloxacin (CIP) antibiotics.
[0038] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a copper-nickel composite catalytic material, characterized in that: The method comprises the following steps: (1) Dissolve 1-3 mmol of Ni(NO3)2•6H2O and 3-5 mmol of Cu(NO3)2•3H2O in a mixed solution of 25 mL of deionized water and 25 mL of ethylene glycol to obtain solution A; 24 mmol of thiourea was dissolved in a mixed solution of 10 mL of deionized water and 10 mL of ethylene glycol to obtain solution B; Solution B was added dropwise into solution A, and after vigorous stirring, the mixture was transferred into a high-pressure reactor for hydrothermal reaction, and a precursor was obtained after the reaction was completed; (2) Washing and drying the obtained precursor, calcining and grinding the dried precursor to obtain a Cu2O(SO4) / NiO composite catalytic material.
2. The method according to claim 1, characterized in that In step (1), 2 mmol of Ni(NO3)2•6H2O and 4 mmol of Cu(NO3)2•3H2O are dissolved in a mixed solution of 25 mL of deionized water and 25 mL of ethylene glycol to obtain solution A.
3. The method according to claim 1, characterized in that In step (1), the temperature of the hydrothermal reaction is 160-200° C. and the time is 20-28 h.
4. The method according to claim 1, characterized in that In step (2), the calcination temperature is 500-800°C, the heating rate is 5°C / min, and the calcination time is 1-4 h.
5. The copper-nickel composite catalytic material prepared by the method according to any one of claims 1 to 4.
6. Use of the copper-nickel composite catalytic material as claimed in claim 5 in activating persulfate to degrade antibiotic pollutants in wastewater.
7. The use according to claim 6, characterized in that The antibiotic pollutant is ciprofloxacin.
Citation Information
Patent Citations
CC-NiO-CuCoS composite material as well as preparation method and application thereof
CN112409028A
Transition metal monatomic active catalyst as well as preparation method and application thereof
CN113600170A
NiFe2S4 material as well as preparation method and application thereof
CN115286047A
ZnO-ZnMnO3 / CuS composite catalytic material as well as preparation method and application thereof
CN117160487A