Biomass carbon-based bifunctional catalyst, preparation method and application of biomass carbon-based bifunctional catalyst in preparation of aldehyde and acetal by oxidizing primary alcohol

By introducing P and B/N atoms into carbon materials and loading metals, a biomass-based carbon bifunctional catalyst was constructed, which solved the problems of difficult product separation and side reactions in the alcohol oxidation process and achieved a highly efficient catalytic effect for one-step conversion of alcohols into aldehydes and acetals.

CN118925758APending Publication Date: 2024-11-12NANJING FORESTRY UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311603466.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-11-28
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing technologies require the addition of homogeneous base or strong acid catalysts in the oxidation of alcohols to aldehydes and acetals, which leads to difficulties in product separation, corrosive hazards, and waste generation. Furthermore, acid and base catalysts cannot be used simultaneously. Research on the one-pot conversion of alcohols to acetals at room temperature and pressure is still lacking.

Method used

A biomass-based carbon bifunctional catalyst was developed by introducing P and B/N atoms into carbon materials and loading metals. By utilizing the synergistic effect of heteroatoms, the coordination state of the metals was changed, and a highly efficient catalyst was constructed to achieve one-step oxidation of alcohols to aldehydes and acetals.

Benefits of technology

It improves catalytic performance and selectivity, avoids side reactions of excessive oxidation of aldehydes, and realizes one-pot conversion of alcohols to acetals. The reaction conditions are mild and have high selectivity and conversion rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925758A_ABST
    Figure CN118925758A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of primary alcohol catalytic oxidation, and particularly relates to a biomass carbon-based bifunctional catalyst, a preparation method and application of the biomass carbon-based bifunctional catalyst in preparation of aldehyde and acetal through primary alcohol oxidation. The biomass carbon-based bifunctional catalyst is obtained by introducing P atoms and B / N atoms into fiber carbon and then carrying out metal loading, through the synergistic effect of heteroatoms, the coordination state of metal is changed, active sites are increased, the catalytic performance and selectivity are enhanced, the side reaction of over-oxidation of aldehyde in the alcohol oxidation process is overcome, and the catalytic activity of the catalyst is improved. The catalyst has better selectivity and conversion rate in one-step oxidation of primary alcohol into aldehyde and acetal, is mild in reaction condition, and has a promising substitute catalyst for one-step conversion of alcohol into aldehyde and acetal.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalytic oxidation of primary alcohols, and in particular relates to a biomass carbon-based bifunctional catalyst, a preparation method and application thereof in the oxidation of primary alcohols to prepare aldehydes and acetals. Background Art

[0002] Aldehydes and acetals are important industrial products. Aldehydes, as high value-added products, are easily oxidized to low value-added acids and esters. Acetals are very stable under neutral and strong alkaline conditions and play an important role in protecting carbonyl groups. This property makes acetals often used as organic intermediates to protect aldehydes or carbonyl groups in organic synthesis. In addition to being used as protecting groups, acetals can also be used as flavoring agents, flavor enhancers, and even as additives in biodiesel.

[0003] At present, in most studies on the oxidation of alcohols into aldehydes, additional homogeneous bases are required to assist in catalysis. At the same time, the method of converting aldehydes into acetals mainly uses strong acids as catalysts. The addition of acids and bases will produce a large amount of waste, and lead to problems such as difficulty in separating products and corrosive hazards. Most importantly, acids and bases cannot be used at the same time. Therefore, there is still a gap in the research on the one-pot conversion of alcohols into acetals at room temperature and pressure.

[0004] Carbon materials have the advantages of low price, stable structure, adjustable electronic structure, etc., and can be synthesized from biomass as a carbon source through pyrolysis. Currently, they have been widely developed as catalysts for many chemical reactions such as organic synthesis, electrochemistry and photocatalysis. Based on this, the present invention discloses a novel catalyst with synergistic effects of metal, phosphorus and nitrogen / boron, which has good catalytic activity in catalyzing the one-step oxidation of alcohol to acetal. Summary of the invention

[0005] In view of the above problems existing in the prior art, the object of the present invention is to provide a biomass carbon-based bifunctional catalyst, a preparation method and its application in the oxidation of primary alcohols to prepare aldehydes and acetals.

[0006] In order to solve the above problems, the technical solution adopted by the present invention is as follows: A method for preparing a biomass carbon-based bifunctional catalyst comprises the following steps: S1, adding a carbon source and a doping source containing B or N into a phosphoric acid solution, stirring to obtain a mixed solution, drying the mixed solution, and then calcining at 400-800° C. for 2-6 h in an inert gas atmosphere to obtain a solid 1; S2, dissolving solid 1 in a hydrochloric acid solution, treating at 110-130° C. for 4-6 h, filtering, washing, and drying to obtain a doped carbon material; S3, dispersing the doped carbon material in water, adding a metal source, stirring for 10-18 h, then heating to 60-70°C and stirring for 4-6 h, then filtering, washing, and drying, and calcining at 200-400°C for 3-6 h to obtain the biomass carbon-based bifunctional catalyst.

[0007] Optionally, the carbon source is one or more of cellulose and glucose.

[0008] Optionally, the doping source is one or more of borax and melamine.

[0009] Optionally, the mass ratio of the carbon source to the doping source is 10:(1-6).

[0010] Optionally, the metal source is one or more of tetraaminopalladium nitrate, chloroplatinic acid, tetrachloroplatinic acid, rhodium chloride, cobalt nitrate hexahydrate, and iron nitrate nonahydrate.

[0011] Optionally, the mass fraction of the metal in the metal source to the doped carbon material is 0.2-5%.

[0012] The biomass carbon-based bifunctional catalyst is prepared according to the above method.

[0013] The above-mentioned biomass carbon-based bifunctional catalyst is used in the oxidation of primary alcohols to prepare aldehydes and acetals. The catalyst is mixed with the primary alcohol, added to a solvent, and reacted at 0-180°C for 1-24 hours; preferably, the reaction is carried out at 50-60°C for 3-6 hours.

[0014] Optionally, the primary alcohol is one or more of benzyl alcohol, phenylethyl alcohol, 2-methylbenzyl alcohol, 3-methylbenzyl alcohol, 4-methylbenzyl alcohol, 2-hydroxybenzyl alcohol, 3-hydroxybenzyl alcohol, 4-hydroxybenzyl alcohol, 2-methoxybenzyl alcohol, 3-methoxybenzyl alcohol, 4-methoxybenzyl alcohol, 2-chlorobenzyl alcohol, 3-chlorobenzyl alcohol, 4-chlorobenzyl alcohol, 2-fluorobenzyl alcohol, 3-fluorobenzyl alcohol, 4-fluorobenzyl alcohol, 3,4-dimethoxybenzyl alcohol, vanillyl alcohol, cinnamyl alcohol, furfuryl alcohol, 5-hydroxymethylfurfural, 1-naphthalenemethanol, 2-naphthalenemethanol, ethanol, n-propanol, n-butanol, n-pentanol, and n-hexanol; and the solvent is one or more of methanol, ethanol, n-propanol, ethylene glycol, 1,3-propylene glycol, 1,2-propylene glycol, acetonitrile, n-hexane, cyclohexane, or the primary alcohol itself.

[0015] Optionally, the mass ratio of the primary alcohol to the catalyst is 1:(0.1-1.5), and the mass ratio of the primary alcohol to the solvent is 1:(10-300).

[0016] Compared with the prior art, the present invention has the following beneficial effects: The present invention introduces P atoms and B / N atoms into fiber carbon, and then loads metal, changes the coordination state of the metal through the synergistic effect of heteroatoms, increases active sites, and enhances catalytic performance and selectivity; constructs a carbon-based bifunctional catalyst containing metal, P and B / N, overcomes the side reaction of over-oxidation of aldehydes during alcohol oxidation, and realizes the one-pot conversion of alcohol to acetal. The present invention proposes a high-efficiency catalyst obtained by loading metal onto P and B / N-doped carbon-based materials, which has better selectivity and conversion rate in realizing one-step oxidation of primary alcohol to aldehyde and acetal, and mild reaction conditions, and will become a promising alternative catalyst for one-step conversion of alcohol to aldehyde and acetal. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is the GC-MS detection spectrum of the product acetal in Example 1; Figure 2 The XRD diagrams of the biomass carbon-based bifunctional catalyst in Example 1 and the catalyst in Comparative Example 1; Figure 3 This is the XPS graph of the biomass carbon-based bifunctional catalyst in Example 1; Figure 4 This is the HRTEM image of the biomass carbon-based bifunctional catalyst in Example 1.

[0018] Figure 5 This is the GC-MS detection spectrum of the product acetal in Example 4; DETAILED DESCRIPTION The present invention is further described below in conjunction with specific embodiments.

[0019] α-Cellulose: Particle size is 25 μm.

[0020] The product detection method is GCMS method, and p-xylene is added as a reference substance to calibrate the yield of the product and the conversion rate of the substrate. The yield calculation formula is: conversion rate = molar amount of detected substrate / molar amount of actual added substrate, and the result is rounded off without retaining decimal points.

[0021] Example 1 A method for preparing a biomass carbon-based bifunctional catalyst comprises the following steps: 30 g of α-cellulose and 15 g of borax were added to 170 g of 85% phosphoric acid solution, stirred until dissolved, and the resulting liquid was vacuum dried at 100 °C for 1 h, and then calcined at 500 °C for 4 h under a nitrogen atmosphere. The resulting solid was dissolved in 500 mL of 1M hydrochloric acid solution, treated at 120 °C for 6 h, filtered, and washed with water and ethanol for 5 times, and dried to obtain a doped carbon material.

[0022] Take 0.5 g of doped carbon material, disperse it in 40 mL of water, ultrasonically disperse it for 1 h, then add 106 μL of a solution containing 10 wt% tetraamino palladium nitrate, stir overnight; then heat to 60 ° C, keep for 6 h, filter, wash the solid with water and ethanol 3-5 times, and dry at 80 ° C. The obtained solid is calcined at 300 ° C for 5 h to obtain a biomass carbon-based bifunctional catalyst. The XRD, XPS and HRTEM test results of the catalyst are shown in Figure 1. Figure 2-Figure 4 No peak of metal particles was found in its XRD. The valence states of Pd in ​​XPS were mainly +4 and +2, and there was no 0 valence. It can be inferred that the catalyst of the present invention is Pd in ​​a single-atom form. The catalyst of the present invention is a supported catalyst, and its atomic utilization rate is higher.

[0023] The method for oxidizing primary alcohol to acetal using the biomass carbon-based bifunctional catalyst obtained above is specifically as follows: Take 10 mg of catalyst, add 15 mg of benzyl alcohol and 3 mL of methanol, and react at 60 °C for 6 h to obtain benzaldehyde dimethyl acetal with a yield of 100%. The GC-MS detection spectrum of the product is shown in Figure 1 ,from Figure 1 It can be seen that no other by-products are generated and the catalyst has high selectivity.

[0024] Example 2 A method for preparing a biomass carbon-based bifunctional catalyst comprises the following steps: 30 g of α-cellulose and 15 g of borax were added to 170 g of 85% phosphoric acid solution, stirred until dissolved, and the resulting liquid was vacuum dried at 95 °C for 1 h, and then calcined at 600 °C for 4 h under a nitrogen atmosphere. The resulting solid was dissolved in 500 mL of 1M hydrochloric acid solution, treated at 120 °C for 6 h, filtered, washed with water and ethanol 3 times, and dried to obtain a doped carbon material.

[0025] Take 0.5 g of doped carbon material, disperse it in 40 mL of water, ultrasonically disperse it for 1 h, then add 618.88 μL of 10 wt% tetrachloroplatinic acid solution and stir overnight; then heat to 65 °C, keep for 6 h, filter, wash the solid with water and ethanol 3-5 times, and dry at 80 °C. The obtained solid is calcined at 300 °C for 5 h to obtain a biomass carbon-based bifunctional catalyst.

[0026] The method for oxidizing primary alcohol to acetal using the biomass carbon-based bifunctional catalyst obtained above is specifically as follows: Take 10 mg of catalyst, add 15 mg of benzyl alcohol and 3 mL of ethanol, and react at 50 °C for 6 h to obtain benzaldehyde diethyl acetal with a yield of 89%.

[0027] Example 3 A method for preparing a biomass carbon-based bifunctional catalyst comprises the following steps: 30 g of α-cellulose and 15 g of borax were added to 170 g of 85% phosphoric acid solution, stirred until dissolved, and the resulting liquid was vacuum dried at 95 °C for 1 h, and then calcined at 600 °C for 6 h under a nitrogen atmosphere. The resulting solid was dissolved in 100 mL of hydrochloric acid solution, treated at 120 °C for 6 h, filtered, washed with water and ethanol 4 times, and dried to obtain a doped carbon material.

[0028] Take 0.5 g of doped carbon material, disperse it in 40 mL of water, ultrasonically disperse it for 1 h, then add 0.0246 g of cobalt nitrate hexahydrate and stir overnight; then heat to 60 ° C, keep for 6 h, filter, wash the solid with water and ethanol 3-5 times, and dry it at 80 ° C. The resulting solid is calcined at 300 ° C for 5 h to obtain a biomass carbon-based bifunctional catalyst.

[0029] The method for oxidizing primary alcohol to acetal using the biomass carbon-based bifunctional catalyst obtained above is specifically as follows: Take 10 mg of the catalyst, add 15 mg of benzyl alcohol and 3 mL of ethylene glycol, and react at 50 °C for 6 h to obtain 2-phenyl-1,3-ditetrahydrofuran with a yield of 98%.

[0030] Example 4 A method for preparing a biomass carbon-based bifunctional catalyst comprises the following steps: 30 g of α-cellulose and 15 g of melamine were added to 170 g of 85% by mass, stirred until dissolved, and the resulting liquid was vacuum dried at 95 °C for 1 h, and then calcined at 600 °C for 6 h under a nitrogen atmosphere. The resulting solid was dissolved in 100 mL of hydrochloric acid solution, treated at 120 °C for 6 h, filtered, washed with water and ethanol 3-5 times, and dried to obtain a doped carbon material.

[0031] Take 0.5 g of doped carbon material, disperse it in 40 mL of water, ultrasonically disperse it for 1 h, then add 0.0362 g of ferric nitrate nonahydrate and stir overnight; then heat to 60 °C, keep for 6 h, filter, wash the solid three times with water and ethanol, and dry it at 80 °C. The obtained solid is calcined at 300 °C for 5 h to obtain a biomass carbon-based bifunctional catalyst.

[0032] The method for oxidizing primary alcohol to acetal using the biomass carbon-based bifunctional catalyst obtained above is specifically as follows: Take 10 mg of catalyst, add 15 mg of vanillin alcohol and 3 mL of methanol, and react at 80 °C for 6 h to obtain vanillin dimethyl acetal with a yield of 65%. The GC-MS detection spectrum of the product is shown in Figure 5 .

[0033] Example 5 A method for preparing a biomass carbon-based bifunctional catalyst comprises the following steps: 30 g of α-cellulose and 15 g of borax were added to 170 g of 85% phosphoric acid solution, stirred until dissolved, and the resulting liquid was vacuum dried at 100 °C for 1 h, and then calcined at 500 °C for 4 h under a nitrogen atmosphere. The resulting solid was dissolved in 500 mL of 1M hydrochloric acid solution, treated at 120 °C for 6 h, filtered, and washed with water and ethanol for 5 times, and dried to obtain a doped carbon material.

[0034] Take 0.5 g of doped carbon material, disperse it in 40 mL of water, ultrasonically disperse it for 1 h, then add 106 μL of a solution containing 10 wt% tetraaminopalladium nitrate and stir overnight; then heat to 60 °C, keep for 6 h, filter, wash the solid with water and ethanol 3-5 times, and dry it at 80 °C. Calcine the obtained solid at 300 °C for 5 h to obtain a biomass carbon-based bifunctional catalyst.

[0035] The method for oxidizing primary alcohol to aldehyde using the biomass carbon-based bifunctional catalyst obtained above is specifically as follows: Take 10 mg of catalyst, add 15 mg of benzyl alcohol and 3 mL of n-hexane, and react at 60 °C for 3 h to obtain benzaldehyde with a yield of 80%.

[0036] Example 6 A method for preparing a biomass carbon-based bifunctional catalyst comprises the following steps: 30 g of glucose and 10 g of borax were added to 170 g of 85% phosphoric acid solution, stirred until dissolved, and the resulting liquid was vacuum dried at 100 °C for 1 h, and then calcined at 800 °C for 6 h under a nitrogen atmosphere. The resulting solid was dissolved in 500 mL of 1M hydrochloric acid solution, treated at 110 °C for 4 h, filtered, and washed with water and ethanol for 5 times, and dried to obtain a doped carbon material.

[0037] Take 0.5 g of doped carbon material, disperse it in 40 mL of water, ultrasonically disperse it for 1 h, then add 106 μL of a solution containing 10 wt% tetraaminopalladium nitrate and stir overnight; then heat to 70 °C, keep for 4 h, filter, wash the solid 4 times with water and ethanol, and dry it at 80 °C. The resulting solid is calcined at 200 °C for 6 h to obtain a biomass carbon-based bifunctional catalyst.

[0038] The method for oxidizing primary alcohol to acetal using the biomass carbon-based bifunctional catalyst obtained above is specifically as follows: Take 8 mg of catalyst, add 15 mg of benzyl alcohol and 3 mL of methanol, and react at 50 °C for 3 h to obtain benzaldehyde dimethyl acetal with a yield of 92%.

[0039] Example 7 A method for preparing a biomass carbon-based bifunctional catalyst comprises the following steps: 30 g of glucose and 5 g of borax were added to 170 g of 85% phosphoric acid solution, stirred until dissolved, and the resulting liquid was vacuum dried at 100 °C for 1 h, and then calcined at 700 °C for 3 h under a nitrogen atmosphere. The resulting solid was dissolved in 500 mL of 1M hydrochloric acid solution, treated at 130 °C for 5 h, filtered, and washed with water and ethanol for 5 times, and dried to obtain a doped carbon material.

[0040] Take 0.5 g of doped carbon material, disperse it in 40 mL of water, ultrasonically disperse it for 1 h, then add 0.0246 g of cobalt nitrate hexahydrate and stir overnight; then heat to 65 ° C, keep for 5 h, filter, wash the solid 4 times with water and ethanol, and dry it at 80 ° C. The resulting solid is calcined at 400 ° C for 4 h to obtain a biomass carbon-based bifunctional catalyst.

[0041] The method for oxidizing primary alcohol to acetal using the biomass carbon-based bifunctional catalyst obtained above is specifically as follows: Take 5 mg of catalyst, add 15 mg of benzyl alcohol and 3 mL of methanol, and react at 50 °C for 5 h to obtain benzaldehyde dimethyl acetal with a yield of 82%.

[0042] Comparative Example 1 (this comparative example differs from Example 1 in that no borax is added) A method for preparing a biomass carbon-based bifunctional catalyst comprises the following steps: 30 g of α-cellulose was added to 170 g of 85% phosphoric acid solution, stirred until dissolved, and the resulting liquid was vacuum dried at 100 °C for 1 h, and then calcined at 500 °C for 4 h under a nitrogen atmosphere. The resulting solid was dissolved in 500 mL of 1M hydrochloric acid solution, treated at 120 °C for 6 h, filtered, and washed with water and ethanol for 5 times, and dried to obtain a doped carbon material.

[0043] Take 0.5 g of doped carbon material, disperse it in 40 mL of water, ultrasonically disperse it for 1 h, then add 106 μL of a solution containing 10 wt% tetraaminopalladium nitrate and stir overnight; then heat to 60 °C, keep for 6 h, filter, wash the solid with water and ethanol 3-5 times, and dry it at 80 °C. Calcine the obtained solid at 300 °C for 5 h to obtain a biomass carbon-based catalyst.

[0044] The method for oxidizing primary alcohol to acetal using the biomass carbon-based catalyst obtained above is specifically as follows: Take 10 mg of catalyst, add 15 mg of benzyl alcohol and 3 mL of methanol, and react at 60 °C for 6 h to obtain benzaldehyde dimethyl acetal with a yield of 20%.

[0045] Comparative Example 2 (the difference between this comparative example and Example 1 is that Pd metal is replaced by Pt metal) A method for preparing a biomass carbon-based bifunctional catalyst comprises the following steps: 30 g of α-cellulose and 15 g of borax were added to 170 g of 85% phosphoric acid solution, stirred until dissolved, and the resulting liquid was vacuum dried at 100 °C for 1 h, and then calcined at 500 °C for 4 h under a nitrogen atmosphere. The resulting solid was dissolved in 500 mL of 1M hydrochloric acid solution, treated at 120 °C for 6 h, filtered, and washed with water and ethanol for 5 times, and dried to obtain a doped carbon material.

[0046] Take 0.5 g of doped carbon material, disperse it in 40 mL of water, ultrasonically disperse it for 1 h, then add 263 μL of 8 wt% chloroplatinic acid solution and stir overnight; then heat to 60 °C, keep for 6 h, filter, wash the solid with water and ethanol 3-5 times, and dry it at 80 °C. Calcine the obtained solid at 300 °C for 5 h to obtain a biomass carbon-based bifunctional catalyst.

[0047] The method for oxidizing primary alcohol to acetal using the biomass carbon-based bifunctional catalyst obtained above is specifically as follows: Take 10 mg of catalyst, add 15 mg of benzyl alcohol and 3 mL of methanol, and react at 60 °C for 3 h to obtain benzaldehyde dimethyl acetal with a yield of 13%.

[0048] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.

Claims

1. A method for preparing a biomass carbon-based bifunctional catalyst, characterized in that: The following steps are involved: S1, adding a carbon source and a doping source containing B or N into a phosphoric acid solution, stirring to obtain a mixed solution, drying the mixed solution, and then calcining at 400-800° C. for 2-6 h in an inert gas atmosphere to obtain a solid 1; S2, dissolving solid 1 in a hydrochloric acid solution, treating at 110-130° C. for 4-6 h, filtering, washing, and drying to obtain a doped carbon material; S3, dispersing the doped carbon material in water, adding a metal source, stirring for 10-18 h, then heating to 60-70°C and stirring for 4-6 h, then filtering, washing, and drying, and calcining at 200-400°C for 3-6 h to obtain the biomass carbon-based bifunctional catalyst.

2. The method for preparing a biomass carbon-based bifunctional catalyst according to claim 1, characterized in that: The carbon source is one or more of cellulose and glucose.

3. The method for preparing a biomass carbon-based bifunctional catalyst according to claim 1, characterized in that: The doping source is any one or more of borax and melamine.

4. The method for preparing a biomass carbon-based bifunctional catalyst according to claim 1, characterized in that: The mass ratio of the carbon source to the doping source is 10:(1-6).

5. The method for preparing a biomass carbon-based bifunctional catalyst according to claim 1, characterized in that: The metal source is one or more of tetraaminopalladium nitrate, chloroplatinic acid, tetrachloroplatinic acid, rhodium chloride, cobalt nitrate hexahydrate, and ferric nitrate nonahydrate.

6. The method for preparing a biomass carbon-based bifunctional catalyst according to claim 1, characterized in that: The mass fraction of the metal in the metal source to the doped carbon material is 0.2-5%.

7. A biomass carbon-based bifunctional catalyst prepared according to the method of claims 1-6.

8. The use of the biomass carbon-based bifunctional catalyst in the oxidation of primary alcohols to produce aldehydes and acetals according to claim 7, characterized in that: The catalyst is mixed with the primary alcohol, added into a solvent, and reacted at 0-180°C for 1-24 hours.

9. Use of the biomass carbon-based bifunctional catalyst according to claim 8 in the oxidation of primary alcohols to produce aldehydes and acetals, characterized in that: The primary alcohol is one or more of benzyl alcohol, phenylethyl alcohol, 2-methylbenzyl alcohol, 3-methylbenzyl alcohol, 4-methylbenzyl alcohol, 2-hydroxybenzyl alcohol, 3-hydroxybenzyl alcohol, 4-hydroxybenzyl alcohol, 2-methoxybenzyl alcohol, 3-methoxybenzyl alcohol, 4-methoxybenzyl alcohol, 2-chlorobenzyl alcohol, 3-chlorobenzyl alcohol, 4-chlorobenzyl alcohol, 2-fluorobenzyl alcohol, 3-fluorobenzyl alcohol, 4-fluorobenzyl alcohol, 3,4-dimethoxybenzyl alcohol, vanillyl alcohol, cinnamyl alcohol, furfuryl alcohol, 5-hydroxymethylfurfural, 1-naphthalenemethanol, 2-naphthalenemethanol, ethanol, n-propanol, n-butanol, n-pentanol, and n-hexanol; and the solvent is one or more of methanol, ethanol, n-propanol, ethylene glycol, 1,3-propylene glycol, 1,2-propylene glycol, acetonitrile, n-hexane, cyclohexane, or the primary alcohol itself.

10. Use of the biomass carbon-based bifunctional catalyst according to claim 8 in the oxidation of primary alcohols to produce aldehydes and acetals, characterized in that: The mass ratio of the primary alcohol to the catalyst is 1:(0.1-1.5), and the mass ratio of the primary alcohol to the solvent is 1:(10-300).