Eutectic molecular sieve catalyst as well as preparation method and application thereof

The ZSM-5/ZSM-11 eutectic molecular sieve is equipped with a solid-loaded heteropolyacid catalyst to catalyze the synthesis of tetrahydrofuran into tetrahydropyrrole in a fixed bed reactor, which solves the problem that powder catalysts are difficult to achieve industrial production in the prior art, and improves the reaction Selectivity and yield, suitable for industrial production.

CN118925788APending Publication Date: 2024-11-12DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310537616.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, it is difficult to achieve industrial production of tetrahydropyrrole in powdered catalysts, and the reaction equipment is required.

Method used

ZSM-5/ZSM-11 eutectic molecular sieve is used as a catalyst and is placed in a fixed bed reactor after forming to catalyze the synthesis of tetrahydrofuran to improve the selectivity and yield of the reaction.

Benefits of technology

It realizes high selectivity and yield of tetrahydropyrrole, simplifies the device, facilitates operation, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004227640470000071
    Figure BDA0004227640470000071
Patent Text Reader

Abstract

The invention discloses a eutectic molecular sieve catalyst as well as a preparation method and application thereof. The eutectic molecular sieve comprises a ZSM-5 / ZSM-11 eutectic molecular sieve and heteropoly acid; the heteropoly acid is immobilized on the ZSM-5 / ZSM-11 eutectic molecular sieve. The ZSM-5 / ZSM-11 eutectic molecular sieve supported heteropolyacid sample is used as the catalyst for catalytic amination of tetrahydrofuran on a fixed bed reactor to synthesize tetrahydropyrrole, and the method has the advantages of simple device, simple operation, easily available raw materials, high selectivity of the target product tetrahydropyrrole and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a eutectic molecular sieve catalyst and a preparation method and application thereof, belonging to the field of catalyst preparation. Background Art

[0002] Tetrahydropyrrole is an important intermediate of fine chemicals, which is widely used in organic synthesis, medicine, pesticides, coatings, daily chemicals and other fields. Tetrahydropyrrole can be used to synthesize dozens of drugs such as buflomedil, dextromorphamide tartrate, procyclidine, procyclidine, and carmatelin; Tetrahydropyrrole can be used to synthesize insecticides such as dicamba; Tetrahydropyrrole reacts with aldehydes, ketones and other compounds to generate enamine compounds; Tetrahydropyrrole is an important solvent in the fine chemical and pharmaceutical industries; Tetrahydropyrrole is an organic template for synthesizing molecular sieves such as ZSM-5, ZSM-35, and ZSM-48; In addition, tetrahydropyrrole can also be used as a desulfurizer, additive and other fine chemical raw materials.

[0003] Tetrahydropyrrole can be synthesized from raw materials such as 1,4-butanediol, 1,4-succinonitrile, 1,4-butanediamine, and tetrahydrofuran. Among them, the synthesis of tetrahydropyrrole by catalytic amination of 1,4-butanediol and tetrahydrofuran has the advantages of simple reaction process, low raw material cost, and high atomic utilization rate, and has high industrial application value.

[0004] However, in the prior art, catalysts are mainly in powder form, and the selectivity and yield of the reaction are improved by increasing the active components of the catalyst. However, the powdered catalyst has high requirements for the reaction equipment, making it difficult to achieve industrial production of tetrahydropyrrole. Summary of the invention

[0005] The present application uses a ZSM-5 / ZSM-11 eutectic molecular sieve immobilized heteropoly acid sample as a catalyst, and places the formed catalyst on a fixed bed reactor to catalyze the amination of tetrahydrofuran to synthesize tetrahydropyrrole, which not only improves the selectivity and yield of tetrahydropyrrole, but also enables the industrialization of the reaction for preparing tetrahydropyrrole.

[0006] According to one aspect of the present application, a eutectic molecular sieve catalyst is provided, comprising a ZSM-5 / ZSM-11 eutectic molecular sieve and a heteropoly acid;

[0007] The heteropoly acid is immobilized on the ZSM-5 / ZSM-11 eutectic molecular sieve.

[0008] Optionally, the heteropoly acid is selected from at least one of phosphotungstic acid, silicotungstic acid, phosphomolybdic acid and silicomolybdic acid.

[0009] Optionally, the loading amount of the heteropoly acid in the eutectic molecular sieve catalyst is 1 to 20 wt %.

[0010] Optionally, the loading amount of the heteropolyacid in the eutectic molecular sieve catalyst is selected from any value of 1wt%, 3wt%, 8wt%, 12wt%, 20wt% or a range between two values.

[0011] Optionally, the specific surface area of ​​the ZSM-5 / ZSM-11 eutectic molecular sieve is 400 to 480 m 2 / g;

[0012] The micropore volume of the ZSM-5 / ZSM-11 eutectic molecular sieve is 0.110-0.140 cm 3 / g;

[0013] The total pore volume of the ZSM-5 / ZSM-11 eutectic molecular sieve is 0.250 to 0.500 cm 3 / g.

[0014] According to another aspect of the present application, a method for preparing a eutectic molecular sieve catalyst is provided, comprising the following steps:

[0015] 1) mixing a mixture containing eutectic molecular sieve raw powder, a binder, and sesbania powder with an acid solution, forming, calcining I, ion exchanging, and calcining II to obtain a formed ZSM-5 / ZSM-11 eutectic molecular sieve;

[0016] 2) The ZSM-5 / ZSM-11 eutectic molecular sieve is immersed in a heteropolyacid solution and calcined III to obtain the eutectic molecular sieve catalyst.

[0017] Optionally, in step 2), the heteropoly acid in the heteropoly acid solution is selected from at least one of phosphotungstic acid, silicotungstic acid, phosphomolybdic acid and silicomolybdic acid.

[0018] Optionally, the mass of the heteropolyacid solution is 1 to 20 wt % of the mass of the ZSM-5 / ZSM-11 eutectic molecular sieve, and the mass of the heteropolyacid solution is calculated based on the mass of the heteropolyacid.

[0019] Optionally, the calcination conditions of III are: in an oxygen-containing atmosphere, heating to 300-500° C. at a heating rate of 0.5-3° C. / min, and keeping the temperature for 1-5 hours.

[0020] Optionally, in step (1), the molar ratio of silicon dioxide to aluminum oxide in the eutectic molecular sieve raw powder is 15 to 500.

[0021] Optionally, the mass ratio of the eutectic molecular sieve raw powder to the adhesive is 0.05 to 19:1.

[0022] Optionally, the mass of the sesbania powder is 0.1 to 15 wt % of the total mass of the eutectic molecular sieve raw powder and the adhesive.

[0023] Optionally, the mass of the acid solution is 10 to 70 wt % of the total mass of the eutectic molecular sieve and the adhesive.

[0024] Optionally, the concentration of the acid solution is 1-8 wt %.

[0025] Optionally, in step 1), the adhesive is pseudo-boehmite.

[0026] Optionally, the acid in the acid solution is selected from nitric acid.

[0027] Optionally, the content of ZSM-5 in the ZSM-5 / ZSM-11 eutectic molecular sieve is 0% to 99.5%, and the content of ZSM-11 is 0.5% to 100%.

[0028] Optionally, the calcination conditions I are: in an oxygen-containing atmosphere, heating to 440-600° C. at a heating rate of 0.5-3° C. / min, and keeping the temperature for 3-24 hours.

[0029] Optionally, the calcination II conditions are: in an oxygen-containing atmosphere, heating to 420-550° C. at a heating rate of 0.5-3° C. / min, and keeping the temperature for 1-5 hours.

[0030] Optionally, the forming method includes extrusion or ball rolling.

[0031] Optionally, the exchange solution for the ion exchange is selected from at least one of oxalic acid, hydrochloric acid, ammonium chloride and ammonium nitrate.

[0032] Optionally, the temperature of the ion exchange is 50 to 95° C., and the time of the ion exchange is 0.5 to 24 hours.

[0033] In the present application, drying is performed before calcination I, calcination II and calcination III, the drying temperature is 60 to 130° C., and the drying time is 6 to 12 hours.

[0034] According to another aspect of the present application, there is provided an application of a eutectic molecular sieve catalyst in the preparation of tetrahydropyrrole by amination of tetrahydrofuran, comprising the following steps:

[0035] The raw material containing tetrahydrofuran and ammonia is contacted with a eutectic molecular sieve catalyst to react and obtain a tetrahydropyrrole product.

[0036] Optionally, the reaction pressure is 0-3 MPa, and the reaction temperature is 160-450°C.

[0037] In the present application, "0 MPa" means a normal pressure state.

[0038] Optionally, the reaction pressure is selected from any value of 0 MPa, 0.5 MPa, 1.0 MPa, 1.5 MPa, 2.0 MPa, 2.5 MPa, 2.8 MPa, 3.0 MPa, or a range between two values.

[0039] Optionally, the reaction temperature is selected from any value of 160°C, 200°C, 220°C, 260°C, 310°C, 320°C, 360°C, 380°C, 400°C, 450°C, or a range between two values.

[0040] Optionally, the space velocity of tetrahydrofuran is 0.02 to 2.0 h -1 .

[0041] Optionally, the space velocity of the tetrahydrofuran is selected from 0.02h -1 、0.08h -1 、0.5h -1 , 1.0h -1 , 1.5h -1 , 1.8h -1 , 2.0h -1 Any value or a range of values ​​between .

[0042] Optionally, the molar ratio of ammonia to tetrahydrofuran in the raw material is 2-20.

[0043] Optionally, the molar ratio of ammonia to tetrahydrofuran in the raw material is selected from any value among 2, 4, 6, 8, 10, 14, 18, 20 or a range value between two values.

[0044] As a specific method for preparing a eutectic catalyst, the method comprises the following steps:

[0045] 1. Fully mix the raw materials containing ZSM-5 / ZSM-11 eutectic molecular sieve powder, binder, and sesbania powder with dilute nitric acid to form a mixture, wherein the content of each component is:

[0046] a) The content of ZSM-5 molecular sieve in the ZSM-5 / ZSM-11 eutectic molecular sieve is 0% to 99.5%, the content of ZSM-11 molecular sieve is 0.5% to 100%, and the sum of the content of ZSM-5 molecular sieve and the content of ZSM-11 molecular sieve is 100%.

[0047] b) The molar ratio of silicon dioxide to aluminum oxide in the ZSM-5 / ZSM-11 eutectic molecular sieve raw powder is 15 to 500.

[0048] c) The specific surface area of ​​ZSM-5 / ZSM-11 eutectic molecular sieve is greater than 400m 2 / g, micropore volume is greater than 0.110cm 3 / g, total pore volume greater than 0.250cm3 / g;

[0049] d) The mass ratio of ZSM-5 / ZSM-11 eutectic molecular sieve raw powder to binder pseudo-boehmite is 0.05-19:1;

[0050] e) the mass of sesbania powder is 0.1 to 15.0 wt % of the total mass of ZSM-5 / ZSM-11 eutectic molecular sieve powder and binder;

[0051] f) the mass of the dilute nitric acid solution is 10-70wt% of the total mass of the ZSM-5 / ZSM-11 eutectic molecular sieve powder and the binder;

[0052] g) the concentration of the dilute nitric acid solution is 1 to 8 wt%;

[0053] 2. Slowly raise the temperature by 0.5-3°C / min to 440-600°C under flowing air and maintain for 3-24 hours to remove the organic template;

[0054] 3. After the calcined sample is exchanged with oxalic acid, hydrochloric acid, ammonium chloride or ammonium nitrate solution, it is dried at 60-130°C for 6-12 hours;

[0055] 4. The exchanged sample is slowly heated to 420-550°C at 0.5-3°C / min under a flowing air atmosphere and maintained for 1-5 hours to obtain a hydrogen sample.

[0056] 5. Add hydrogen molecular sieve into heteropoly acid solution, stir thoroughly and dry;

[0057] 6. The hydrogen-type molecular sieve sample impregnated with the heteropolyacid solution is slowly heated to 300-500° C. by 0.5-3° C. / min under a flowing air atmosphere and maintained for 1-5 hours to obtain a eutectic molecular sieve-supported heteropolyacid catalyst.

[0058] The beneficial effects of this application include:

[0059] 1) The ZSM-5 / ZSM-11 eutectic molecular sieve supported heteropoly acid catalyst provided in the present application has excellent catalytic performance in the amination reaction of tetrahydrofuran to prepare tetrahydropyrrole, with a conversion rate of tetrahydrofuran greater than 88%, a selectivity of tetrahydropyrrole greater than 78%, and a yield of tetrahydropyrrole greater than 71%.

[0060] 2) The ZSM-5 / ZSM-11 eutectic molecular sieve supported heteropoly acid catalyst provided in the present application is a formed solid catalyst, reacts in a fixed bed reactor, has a simple device, is easy to operate, and can be used for the industrial production of tetrahydropyrrole.

[0061] 3) The raw materials for the amination of tetrahydrofuran to prepare tetrahydropyrrole provided in the present application are readily available. DETAILED DESCRIPTION

[0062] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0063] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.

[0064] The analysis method in the examples of this application is as follows:

[0065] Tetrahydrofuran conversion rate = (tetrahydrofuran carbon moles in reactants - tetrahydrofuran carbon moles in products) / tetrahydrofuran carbon moles in reactants × 100%

[0066] Tetrahydropyrrole selectivity = mole number of tetrahydropyrrole carbon in the product / (mole number of tetrahydrofuran carbon in the reactant - mole number of tetrahydrofuran carbon in the product) × 100%

[0067] Tetrahydropyrrole yield = mole number of tetrahydropyrrole carbon in the product / mole number of tetrahydrofuran carbon in the reactant × 100%

[0068] In the examples of the present application, the tetrahydrofuran conversion, tetrahydropyrrole selectivity and tetrahydropyrrole yield are all calculated based on the carbon molar number.

[0069] Example 1

[0070] 11.36g ZSM-5 / ZSM-11 eutectic molecular sieve raw powder (dry basis 88%, ZSM-5 content 95%, silica to alumina molar ratio of 400), 116.13g pseudo-boehmite (dry basis 77.5%), 12.00g sesbania powder, 20.00g dilute nitric acid solution with a mass concentration of 6.5wt% were fully mixed and formed by extrusion. Dry at 80°C for 12h. Then, heat to 580°C at 1.5°C / min and keep for 4h to remove the organic template. Ion exchange was performed with 0.8mol / L ammonium nitrate solution and repeated three times. After drying at 120°C, heat to 530°C at 1.5°C / min and keep for 4h. Thus, a columnar catalyst material with a ZSM-5 / ZSM-11 eutectic molecular sieve content of 10% was obtained.

[0071] The surface area of ​​ZSM-5 / ZSM-11 eutectic molecular sieve is 405m 2 / g, micropore volume is 0.120cm 3 / g, with a total pore volume of 0.260 cm 3 / g.

[0072] 3.00g of phosphotungstic acid was added to 55.00g of water, stirred and dissolved. Then 97.00g of the above columnar catalyst material was added, stirred and dried at 80°C for 10h, and then heated to 420°C at 2.0°C / min and kept for 2h. Thus, a ZSM-5 / ZSM-11 eutectic molecular sieve immobilized phosphotungstic acid catalyst with a phosphotungstic acid immobilization amount of 3% was obtained, which was recorded as catalyst A.

[0073] Example 2

[0074] 51.14g ZSM-5 / ZSM-11 eutectic molecular sieve raw powder (dry basis 88%, ZSM-5 content 55%, silica to alumina molar ratio of 25), 70.97g pseudo-boehmite (dry basis 77.5%), 8.00g sesbania powder, 60.00g dilute nitric acid solution with a mass concentration of 2.0wt% were fully mixed and formed by rolling. Dry at 90°C for 8h. Then, heat to 460°C at 2.5°C / min and keep for 20h to remove the organic template. Ion exchange was performed with 0.8mol / L oxalic acid solution and repeated three times. After drying at 80°C, heat to 450°C at 2.5°C / min and keep for 2h. Thus, a spherical catalyst material with a ZSM-5 / ZSM-11 eutectic molecular sieve content of 45% was obtained.

[0075] Among them, the specific surface area of ​​ZSM-5 / ZSM-11 eutectic molecular sieve is 430m 2 / g, micropore volume is 0.120cm 3 / g, and the total pore volume is 0.380cm 3 / g.

[0076] 8.00g of silicotungstic acid was added to 70.00g of water, stirred and dissolved. Then 92.00g of the spherical catalyst material was added, stirred and dried at 110°C for 8h, and then heated to 380°C at 1.5°C / min and kept for 4h. Thus, a ZSM-5 / ZSM-11 eutectic molecular sieve-supported silicotungstic acid catalyst with a silicotungstic acid solid loading of 8% was obtained, which was recorded as catalyst B.

[0077] Example 3

[0078] 102.27g ZSM-5 / ZSM-11 eutectic molecular sieve raw powder (dry basis 88%, ZSM-5 content 10%, silica to alumina molar ratio of 60), 12.90g pseudo-boehmite (dry basis 77.5%), 1.50g sesbania powder, 45.00g dilute nitric acid solution with a mass concentration of 4.0wt% were fully mixed and formed by extrusion. Dry at 120°C for 8h. Then, heat to 530°C at 2.0°C / min and keep for 6h to remove the organic template. Ion exchange was performed with 0.8mol / L ammonium chloride solution and repeated three times. After drying at 80°C, heat to 510°C at 2.0°C / min and keep for 3h. Thus, a columnar catalyst material with a ZSM-5 / ZSM-11 eutectic molecular sieve content of 90% was obtained.

[0079] Among them, the specific surface area of ​​ZSM-5 / ZSM-11 eutectic molecular sieve is 470m 2 / g, micropore volume is 0.130cm 3 / g, and the total pore volume is 0.480cm 3 / g.

[0080] 12.00 g of phosphomolybdic acid was added to 90.00 g of water, stirred and dissolved. Then 88.00 g of the above columnar catalyst material was added, stirred and dried at 90° C. for 10 h, and then heated to 400° C. at 1.8° C. / min and maintained for 3 h. Thus, a ZSM-5 / ZSM-11 eutectic molecular sieve-supported phosphomolybdic acid catalyst with a phosphomolybdic acid solid loading of 12% was obtained, which was recorded as catalyst C.

[0081] Example 4

[0082] The catalytic performance of the prepared catalyst in the amination of tetrahydrofuran to tetrahydropyrrole was evaluated in a fixed bed reactor. The reactor diameter was 13 mm, the catalyst loading was 3 g, the reaction pressure was 0.0-3.0 MPa (0.0 MPa represents normal pressure), the reaction temperature was 160-450°C, and the tetrahydrofuran space velocity was 0.02-2.0 h -1 , the ammonia / tetrahydrofuran molar ratio is 2 to 20.

[0083] The reaction results are shown in Table 1.

[0084] Table 1 Catalytic performance of the catalyst of the present invention in the reaction of tetrahydrofuran amination to tetrahydropyrrole

[0085]

[0086] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A eutectic molecular sieve catalyst, characterized in that: Including ZSM-5 / ZSM-11 eutectic molecular sieve and heteropoly acid; The heteropoly acid is immobilized on the ZSM-5 / ZSM-11 eutectic molecular sieve.

2. The eutectic molecular sieve catalyst according to claim 1, characterized in that: The heteropoly acid is selected from at least one of phosphotungstic acid, silicotungstic acid, phosphomolybdic acid and silicomolybdic acid; Preferably, the loading amount of the heteropoly acid in the eutectic molecular sieve catalyst is 1 to 20 wt%; Preferably, the specific surface area of ​​the ZSM-5 / ZSM-11 eutectic molecular sieve is 400 to 480 m 2 / g; The micropore volume of the ZSM-5 / ZSM-11 eutectic molecular sieve is 0.110 to 0.140 cm 3 / g; The total pore volume of the ZSM-5 / ZSM-11 eutectic molecular sieve is 0.250 to 0.500 cm 3 / g.

3. A method for preparing the eutectic molecular sieve catalyst according to claim 1 or 2, characterized in that: The following steps are involved: 1) mixing a mixture containing eutectic molecular sieve raw powder, a binder, and sesbania powder with an acid solution, forming, calcining I, ion exchanging, and calcining II to obtain a formed ZSM-5 / ZSM-11 eutectic molecular sieve; 2) The ZSM-5 / ZSM-11 eutectic molecular sieve is immersed in a heteropolyacid solution and calcined III to obtain the eutectic molecular sieve catalyst.

4. The preparation method according to claim 3, characterized in that: In step 2), the heteropoly acid in the heteropoly acid solution is selected from at least one of phosphotungstic acid, silicotungstic acid, phosphomolybdic acid and silicomolybdic acid; Preferably, the mass of the heteropoly acid solution is 1 to 20 wt % of the mass of the ZSM-5 / ZSM-11 eutectic molecular sieve, and the mass of the heteropoly acid solution is calculated based on the mass of the heteropoly acid; Preferably, the calcination conditions of III are: in an oxygen-containing atmosphere, heating to 300-500° C. at a heating rate of 0.5-3° C. / min, and keeping the temperature for 1-5 hours.

5. The preparation method according to claim 3, characterized in that: In step (1), the molar ratio of silicon dioxide to aluminum oxide in the eutectic molecular sieve raw powder is 15 to 500; Preferably, the mass ratio of the eutectic molecular sieve raw powder to the adhesive is 0.05 to 19:1; Preferably, the mass of the sesbania powder is 0.1 to 15 wt % of the total mass of the eutectic molecular sieve raw powder and the adhesive; Preferably, the mass of the acid solution is 10-70wt% of the total mass of the eutectic molecular sieve and the adhesive; Preferably, the concentration of the acid solution is 1-8 wt %.

6. The preparation method according to claim 3, characterized in that: In step 1), the adhesive is pseudo-boehmite; Preferably, the acid in the acid solution is selected from nitric acid; Preferably, the content of ZSM-5 in the ZSM-5 / ZSM-11 eutectic molecular sieve is 0% to 99.5%, and the content of ZSM-11 is 0.5% to 100%.

7. The preparation method according to claim 3, characterized in that: The calcination conditions of I are: in an oxygen-containing atmosphere, heating to 440-600° C. at a heating rate of 0.5-3° C. / min, and keeping the temperature for 3-24 hours; Preferably, the conditions of calcination II are: in an oxygen-containing atmosphere, heating to 420-550° C. at a heating rate of 0.5-3° C. / min, and keeping the temperature for 1-5 hours; Preferably, the forming method includes extrusion or ball rolling.

8. The preparation method according to claim 3, characterized in that: The ion exchange solution is selected from at least one of oxalic acid, hydrochloric acid, ammonium chloride and ammonium nitrate; Preferably, the temperature of the ion exchange is 50-95° C., and the time of the ion exchange is 0.5-24 h.

9. Use of the eutectic molecular sieve catalyst according to claim 1 or 2 in the preparation of tetrahydropyrrole by amination of tetrahydrofuran, characterized in that: The following steps are involved: The raw material containing tetrahydrofuran and ammonia is contacted with a eutectic molecular sieve catalyst to react and obtain a tetrahydropyrrole product.

10. The use according to claim 9, characterized in that: The reaction pressure is 0-3MPa, 0MPa is normal pressure, and the reaction temperature is 160-450°C; Preferably, the space velocity of tetrahydrofuran is 0.02 to 2.0 h -1 ; Preferably, the molar ratio of ammonia to tetrahydrofuran in the raw material is 2-20.