Cracking catalyst containing SAPO-34 molecular sieve as well as preparation method and application of cracking catalyst

By combining nano-scale layered SAPO-34 molecular sieve and ZSM-5 molecular sieve and other materials, a catalyst with a mesoporous structure was prepared, which solved the problem of low ethylene selectivity of SAPO-34 molecular sieve catalyst in naphtha and improved catalysis The selectivity of ethylene, propylene and butene in the cracking reaction improves the selectivity of total low-carbon olefins.

CN118925795APending Publication Date: 2024-11-12CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310523644.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing SAPO-34 molecular sieve catalysts have low selectivity in naphtha conversion of ethylene, and the reactant diffusion resistance is large, which affects the catalytic effect.

Method used

Using nano-scale layered SAPO-34 molecular sieve combined with ZSM-5 molecular sieve, binder and clay, a catalyst with a mesoporous structure is formed through specific preparation methods and treatment steps, and the diffusion performance and activity center utilization of the catalyst are improved. Rate.

Benefits of technology

The selectivity of ethylene, propylene and butene is significantly improved, the selectivity of total low-carbon olefins is improved, and the efficiency of catalytic cracking reaction is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004222099160000051
    Figure BDA0004222099160000051
  • Figure BDA0004222099160000052
    Figure BDA0004222099160000052
  • Figure BDA0004222099160000053
    Figure BDA0004222099160000053
Patent Text Reader

Abstract

The invention belongs to the technical field of catalytic cracking, and relates to a cracking catalyst containing an SAPO-34 molecular sieve as well as a preparation method and application of the cracking catalyst, the catalytic cracking catalyst contains 1 wt%-80 wt% of the SAPO-34 molecular sieve, 0 wt%-50 wt% of a ZSM-5 molecular sieve, 1 wt%-50 wt% of a binder I, 1 wt%-60 wt% of a binder II and 1 wt%-40 wt% of clay; the SAPO-34 molecular sieve is characterized in that the SAPO-34 molecular sieve has nanoscale lamellar crystal grains. The catalyst is used for naphtha catalytic cracking, has high ethylene selectivity, and preferably has high propylene selectivity and butene selectivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalyst preparation, and in particular relates to a preparation method of a catalytic cracking catalyst containing lamellar SAPO-34 molecular sieve and application of the catalyst in a catalytic cracking reaction. Background Art

[0002] With the growing momentum of new energy and renewable energy development, the refined oil market is facing a serious impact, and the problem of structural overcapacity in refining capacity is becoming increasingly serious. At present, the most effective way to resolve the structural overcapacity in refining capacity is to convert part of the excess refining capacity into the production of low-carbon olefins and other chemicals. Low-carbon olefins are the general term for ethylene, propylene, and butene (trienes). Ethylene and propylene (dienes) are representatives of low-carbon olefins. As monomers, they can produce many products and intermediates such as polyethylene, styrene, polypropylene, and propylene oxide. They are very important basic organic chemical raw materials.

[0003] Fluidized catalytic cracking is one of the main processes for producing low-carbon olefins. Studies have shown that small-pore molecular sieves are beneficial to catalytic cracking to increase the production of low-carbon olefins. Among them, the ZSM-5 molecular sieve is recognized to have the best performance and is the most widely used. The ZSM-5 molecular sieve has a special straight pore (0.53nm×0.56nm) and sinusoidal pore (0.51nm×0.55nm) structure, which can crack olefins and alkanes in gasoline components to generate common low-carbon olefins. For example, CN100351345 C discloses a petroleum hydrocarbon catalytic cracking catalyst, which contains 10% to 65% of modified ZSM-5 molecular sieves. The use of this catalyst can increase the yield of catalytic cracking liquefied gas and improve the octane number of catalytic cracking gasoline, and can also significantly increase the propylene concentration in the liquefied gas. Although ZSM-5 can increase the yield of propylene as a commonly used additive, it does not significantly increase the yield of ethylene.

[0004] In recent years, there have been increasing reports on the use of smaller pore size silicoaluminophosphate (SAPO) molecular sieves in catalytic cracking catalysts to produce light olefins. In the early 1980s, Union Carbide Corporation of the United States successfully developed a new molecular sieve system - silicoaluminophosphate (SAPO-n) series molecular sieves, which are composed of phosphorus oxygen tetrahedron (PO4), aluminum oxygen tetrahedron (AlO4) and silicon oxygen tetrahedron (SiO4) to form a three-dimensional framework structure.

[0005] CN1754624A discloses a transition metal-modified SAPO-34 molecular sieve as a catalytically active component in the cracking process of petroleum hydrocarbons, which can improve the yield and selectivity of C2-C4 olefins and has a higher liquefied gas yield.

[0006] CN100569371C discloses a catalytic cracking catalyst, wherein the active components are composed of Y-type molecular sieve, HZSM-5 molecular sieve and SAPO molecular sieve. The catalyst is used in the catalytic cracking process and can convert methanol, ethanol or alcohols and ethers into light olefins while producing petroleum products, so it has a high conversion rate and light olefin selectivity.

[0007] CN 102816588 A discloses a cracking catalyst containing 1 to 90% of a silicoaluminophosphate molecular sieve having an octagonal ring channel structure, which can flexibly adjust the yield of catalytic cracking light olefins and the ratio of olefin product types.

[0008] The kinetic diameter of ethylene is comparable to the diameter of the octagonal ring pores of SAPO-34 molecular sieve, which is beneficial for improving the selectivity of ethylene. However, due to the small size of the pores of SAPO-34 molecular sieve, the diffusion of reactants in it has a large mass transfer resistance, which has an adverse effect on the ethylene selectivity of the catalyst. Summary of the invention

[0009] The technical problem to be solved by the present invention is to provide a catalytic cracking catalyst containing SAPO-34 molecular sieve in view of the problem that the selectivity of naphtha conversion to ethylene in the prior art catalyst containing SAPO-34 molecular sieve is not high. Another technical problem to be solved by the present invention is to provide a preparation method and application method of the cracking catalyst.

[0010] The present invention provides a catalytic cracking catalyst containing SAPO-34 molecular sieve, which contains 1wt% to 80wt% of SAPO-34 molecular sieve, 0wt% to 50wt% of ZSM-5 molecular sieve, 1wt% to 50wt% of binder I, 1wt% to 60wt% of binder II and 1wt% to 40wt% of clay, based on the total dry weight of the catalytic cracking catalyst. Wherein wt% refers to the weight percentage content; the SAPO-34 molecular sieve has nano-scale lamellar grains.

[0011] Preferably, the SAPO-34 molecular sieve has a composition based on oxide moles: 1.0Al2O3: (0.8-1.2)P2O5: (0.2-1.2)SiO2.

[0012] The SAPO-34 molecular sieve has nano-scale lamellar grains, wherein the SAPO-34 molecular sieve grain thickness does not exceed 200nm, such as 20-200nm, and the grain size is less than 1 micron, such as 90-980nm; the grain size refers to the length of the longest side of the rectangle on the surface of the grain perpendicular to the grain thickness direction. The crystal size and thickness are determined by scanning electron micrograph (SEM) measurement, and the measurement method is: 50 grains are randomly selected, and the grain size and thickness are measured by measurement software, and the minimum and maximum values ​​of the grain size and thickness are used as the respective size ranges.

[0013] Preferably, the SAPO-34 molecular sieve also has mesopores, that is, the SAPO-34 molecular sieve is a nanosheet-shaped layered SAPO-34 molecular sieve with mesopores. The mesopore volume of the SAPO-34 molecular sieve accounts for more than 10% of the total pore volume, for example, 13 to 17%. The use of nanosheet-shaped layered SAPO-34 molecular sieves with mesopores has small grains and many mesopores, and has better diffusion performance. It can not only shorten the residence time of the reactant molecules in the pores and improve the intracrystalline diffusion efficiency, but also improve the connectivity between the pores and the outer surface, improve the utilization rate of the active center, and have a better effect of improving the selectivity of ethylene, propylene and butene.

[0014] The catalytic cracking catalyst provided by the present invention may contain 0wt% to 50wt%, such as 0-20wt% of ZSM-5 molecular sieve, and the ZSM-5 molecular sieve may have a higher butene selectivity. Preferably, the ZSM-5 molecular sieve has a SiO2 / Al2O3 molar ratio of not more than 25, such as 15 to 20, a Na2O content of not more than 0.25wt%, such as 0.02wt% to 0.15wt%, a crystallinity of not less than 90%, such as 92% to 97%, and a specific surface area of ​​not less than 300m 2 / gFor example 330m 2 / g~450m 2 / g.

[0015] According to the present invention, the binder I is a binder that performs dispersion and bonding functions on kaolin particles, such as one or more of aluminum sol, silica sol, phosphoaluminum colloid or silica-aluminum sol. The first binder is preferably silica sol, which can have higher ethylene selectivity, higher propylene selectivity and higher butene selectivity. The binder II is a binder that can improve the macromolecular precracking ability and anti-wear performance of the catalyst, such as pseudo-boehmite, which can be one or more of acidified pseudo-boehmite or unacidified pseudo-boehmite.

[0016] According to one embodiment of the present invention, the specific surface area of ​​the catalytic cracking catalyst is 150 to 200 (m 2 / g), the total pore volume is 0.1~0.2(cm3 / g) such as 0.11 to 0.15 (cm 3 / g). The mesopore volume is 0.05 to 0.09, for example, 0.06 to 0.08 (cm 3 / g).

[0017] In the present invention, mesopore volume refers to the volume of pores with a pore diameter in the range of 2 to 50 nm, and total pore volume refers to the volume of pores with a pore diameter in the range of 0 to 100 nm. The pore volume and specific surface area are measured by low-temperature nitrogen physical adsorption BET method, see standard GBT21650.2-2008 and standard GB / T 19587-2004. The pore diameter in the present invention refers to the diameter of the pore.

[0018] Another aspect of the present invention provides a method for preparing the catalytic cracking catalyst, comprising the following steps:

[0019] a) mixing SAPO-34 molecular sieve with water, such as deionized water, and preferably stirring for 0.5 to 8 hours to obtain molecular sieve slurry A;

[0020] b) mixing clay, binder I and water, such as deionized water, and shearing, such as shearing for 0.5 to 4 hours, to obtain a mixed solution B;

[0021] c) mixing the mixed solution B, the molecular sieve slurry A and the binder II, and shearing them, for example, for 0.5 to 4 hours, to obtain a mixed solution C;

[0022] d) spray drying the mixed solution C to prepare a microsphere catalyst; and post-treating the microsphere catalyst to obtain a catalytic cracking catalyst.

[0023] The microsphere catalyst is post-treated. In one embodiment, the microsphere catalyst is calcined at 500°C for 1 to 10 hours, washed, for example, with (NH4)2SO4 solution at 20 to 80°C until the Na2O content is less than 0.25wt%, then rinsed with water, for example, deionized water and filtered, and then dried, for example, at 110°C.

[0024] In the preparation method of the catalytic cracking catalyst, the binder I is selected from one or more of aluminum sol, silica sol, phosphate aluminum colloid or silica aluminum sol; the binder II is selected from one or more of pseudo-boehmite, such as acidified pseudo-boehmite or unacidified pseudo-boehmite, the molar ratio of acid to alumina in the acidified pseudo-boehmite is 0.1-0.3, such as 0.15-0.25, and the acid is such as one of hydrochloric acid and nitric acid; the clay is selected from one or more of kaolin, such as halloysite, montmorillonite or diatomaceous earth.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] The catalytic cracking catalyst provided by the present invention is used for naphtha conversion, has higher ethylene selectivity, and can have higher butene selectivity. Preferably, when the SAPO-34 is a SAPO-34 molecular sieve in the form of small crystals containing mesopores, it can have higher ethylene selectivity, higher butene selectivity, and can have higher total light olefins (ethylene+propylene+butene) selectivity compared with the existing SAPO-34 molecular sieve.

[0027] The catalyst cracking catalyst provided by the invention is used for naphtha catalytic cracking reaction and can improve the ethylene selectivity in the product.

[0028] The catalytic cracking catalyst is suitable for catalytic cracking of naphtha, comprising the step of contacting naphtha with the catalytic cracking catalyst for reaction. Preferably, the reaction temperature is 550-650°C, and the weight hourly space velocity is 2-10h -1 For example, 4-8 hours -1 The agent-oil ratio is preferably 6 to 10 by weight. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is the SEM image of the nano-scale lamellar SAPO-34 molecular sieve prepared in Example 1.

[0030] Figure 2 This is a graph showing the N2 physical adsorption-desorption curve of the nano-scale lamellar SAPO-34 molecular sieve prepared in Example 1. DETAILED DESCRIPTION

[0031] In one embodiment, the SAPO-34 molecular sieve has a mesoporous structure, and the mesoporous volume of the SAPO-34 molecular sieve accounts for more than 10% of the total pore volume. A method for synthesizing a small-grain SAPO-34 molecular sieve with mesopores comprises the following steps:

[0032] (1) mixing an aluminum source, a template agent I and water, stirring for 0 to 30 minutes, then adding a template agent II, and mixing uniformly to obtain a mixed solution A; the mixing uniformly is, for example, stirred at room temperature for 1 to 10 hours, and the room temperature is 20 to 30° C.;

[0033] wherein the molar ratio of template I:template II is 0.25 to 4:1, for example, 0.25 to 2.5:1, and the molar ratio of the total amount of template I and template II to the aluminum source calculated as Al2O3 is 1 to 4:1;

[0034] The template agent I is a template agent that has the function of forming a CHA cage and filling a microporous structure, and the template agent II is a template agent that is easily adsorbed on the crystal surface of the grain and has the function of inhibiting the growth of the crystal surface;

[0035] (2) adding a phosphorus source to the mixed solution A and stirring the mixture evenly, for example, for 1 to 10 hours at room temperature, to obtain a mixed solution B;

[0036] (3) Adding a silicon source to the mixed solution B and stirring the mixture evenly, for example, for more than 0.5 h, to obtain a mixed solution C;

[0037] (4) hydrothermal dynamic crystallization of the mixed solution C at 150-220° C. for 12-120 h;

[0038] (5) separating, washing, and drying to obtain a solid product;

[0039] (6) Calcination; the calcination is, for example, at 450-600° C. for 2-8 hours.

[0040] The method for synthesizing small-grain SAPO-34 molecular sieve with mesopores obtains a SAPO-34 molecular sieve with mesopores and a nanosheet layered structure.

[0041] The method for synthesizing small-grain SAPO-34 molecular sieve with mesopores, wherein the silicon source is selected from one or more of silica sol, silicon dioxide, white carbon black or tetraethyl orthosilicate; the aluminum source is selected from one or more of boehmite, pseudo-boehmite, alumina, aluminum hydroxide or aluminum isopropoxide; the phosphorus source is one or more of phosphoric acid, phosphorous acid, ammonium dihydrogen phosphate or diammonium hydrogen phosphate, preferably phosphoric acid; the template agent I is selected from one or more of tetraethylammonium hydroxide, tetraethylammonium chloride or tetraethylammonium bromide; the template agent II is selected from one or more of diethylamine, triethylamine, morpholine or isopropylamine.

[0042] In the synthesis method of small-grain SAPO-34 molecular sieve with mesopores, in one embodiment, the amount of each material is such that the mixed solution C has the following molar ratio:

[0043] SiO2:Al2O3=0.2~1.2; P2O5:Al2O3=0.8~1.2; Template I:Al2O3=0.2~1.8; Template

[0044] II:Al2O3=0.2~1.8; H2O:Al2O3=20~100.

[0045] Preferably, the value of template I: Al2O3 is 0.2-0.8, and the value of template II: Al2O3 is, for example, 0.4-1.2; (template I+

[0046] Template II): Al2O3 = 1 to 2, and the above ratios are all molar ratios.

[0047] Preferably, in the method for synthesizing small-grain SAPO-34 molecular sieve with mesopores, in step (1), after the aluminum source and template agent I are mixed, they are stirred for 0-30 minutes, for example, 5-20 minutes, and template agent II is added; wherein water can be added before the aluminum source and template agent, or added at the same time as the aluminum source and template agent I, or added after the aluminum source and template agent I.

[0048] The following examples will further illustrate the present invention and are intended to help readers better understand the essence of the present invention and the beneficial effects brought about, but should not be construed as any limitation on the practicable scope of the present invention.

[0049] The ZSM-5 molecular sieve was purchased from the catalyst plant of Nankai University, with a SiO2 / Al2O3 molar ratio of 18.4, a N2O content of 0.04 wt%, a crystallinity of 96%, and a specific surface area of ​​350 m 2 / g.

[0050] Pseudo-boehmite (used for SAPO-34 molecular sieve synthesis), China Aluminum Shanxi New Materials Co., Ltd., with an Al2O3 content of 72.6% by weight.

[0051] Silica sol, Qingdao Jiyida Silica Gel Reagent Co., Ltd., SiO2 content 40% by weight, pH 9.4.

[0052] Tetraethylammonium hydroxide solution, Beijing Inokai Technology Co., Ltd., content 25% by weight.

[0053] Triethylamine, Beijing Inokai Technology Co., Ltd., purity 99.5%.

[0054] Phosphoric acid solution, Tianjin Damao Chemical Reagent Factory, phosphoric acid content 85 wt%.

[0055] Fumed silica, McLean Biological Reagents Co., Ltd., surface area 200 m 2 / g.

[0056] Kaolin, solid content 85% by weight, Suzhou Kaolin Company.

[0057] Pseudo-boehmite (for catalyst preparation), Al2O3 content 62% by weight, manufacturer: Shandong Aluminum Plant. Acidified pseudo-boehmite (abbreviated as acidified diaspore), solid content 60% by weight, according to the acid-aluminum ratio (HCl: Al2O3 molar ratio) of 0.2, acidified with hydrochloric acid.

[0058] Alumina sol, Al2O3 content 22% by weight, manufacturer: Hunan Xinpeng Petrochemical Co., Ltd., Cl / Al molar ratio 0.1.

[0059] Synthesis of SAPO-34 Molecular Sieve

[0060] Molecular sieve synthesis example 1

[0061] 13.00g pseudo-boehmite and 76.20g tetraethylammonium hydroxide solution were added to 26.97g ionized water, stirred at 25°C for 10min, then 5.61g triethylamine was added, and the mixture was stirred for 2h to obtain a mixed solution A; 21.35g phosphoric acid solution was added to the mixed solution A, and the mixture was stirred at 25°C for 2h to obtain a mixed solution B; 6.87g silica sol was added to the mixed solution B, and the mixture was stirred for 2h to obtain a mixed solution C; the mixed solution C was crystallized at 200°C for 48h, and the speed of the crystallization kettle was 10r / min. After the crystallization was completed, the solid product was centrifuged, washed, and dried to obtain a solid product, i.e., the original molecular sieve powder; then the original molecular sieve powder was calcined at 550°C in air for 5h to remove the template agent, and a nano-scale lamellar SAPO-34 molecular sieve was obtained, which was marked as SP-A sample. The crystal grains of the SP-A sample are lamellar and have a rectangular surface.

[0062]

[0063] Comparative Example 1 of Synthesis of SAPO-34 Molecular Sieve

[0064] 13.54g pseudo-boehmite and 19.47g triethylamine were added to 87.61g deionized water, stirred at 25℃ for 2h, and mixed evenly to obtain mixed solution A; 22.23g phosphoric acid solution was added to mixed solution A, stirred at 25℃ for 1h, and mixed solution B was obtained; 7.15g silica sol was added to mixed solution B, and stirred for 2h, and mixed solution C was obtained; mixed solution C was crystallized at 200℃ for 24h, and the speed of the crystallization kettle was 10r / min. After the crystallization, the solid product, i.e., the original molecular sieve powder, was centrifuged, washed, and dried; then the original molecular sieve powder was calcined at 550℃ in air for 5h to remove the template agent, and SAPO-34 molecular sieve was obtained, which was marked as SP-B sample. The crystal grains of SP-B sample are cubes.

[0065]

[0066] Molecular sieve synthesis example 2

[0067] The lamellar SAPO-34 molecular sieve prepared according to Example 1 of patent CN 104192860 A is marked as SP-C sample.

[0068]

[0069] Catalyst Preparation Example 1

[0070] 60g SAPO-34 molecular sieve (SP-A) was mixed with 180g deionized water and stirred for 1h to obtain molecular sieve slurry A; then 71g kaolin, 182g aluminum sol and 108g deionized water were mixed and sheared for 1h to obtain mixed solution B; molecular sieve slurry A and 67g acidified aluminum stone were added to mixed solution B and sheared for 0.5h to obtain mixed solution C; mixed solution C was spray-dried to prepare a microsphere catalyst, and then the microsphere catalyst was calcined at 500°C for 4h, and then washed with (NH4)2SO4 solution at 60°C until the Na2O content was less than 0.25wt%, followed by rinsing with deionized water and filtering, and then drying at 110°C to obtain a catalytic cracking catalyst, marked as CA sample.

[0071] Catalyst Preparation Example 2

[0072] 80g SAPO-34 molecular sieve (SP-A) was mixed with 240g deionized water and stirred for 1h to obtain molecular sieve slurry A; then 59g kaolin, 136g aluminum sol and 85g deionized water were mixed and sheared for 1h to obtain mixed solution B; molecular sieve slurry A and 67g acidified aluminum stone were added to mixed solution B and sheared for 0.5h to obtain mixed solution C; mixed solution C was spray-dried to prepare a microsphere catalyst, and then the microsphere catalyst was calcined at 500°C for 4h, and then washed with (NH4)2SO4 solution at 60°C until the Na2O content was less than 0.25wt%, followed by rinsing with deionized water and filtering, and then drying at 110°C to obtain a catalytic cracking catalyst, marked as CB sample.

[0073] Catalyst Preparation Example 3

[0074] 60g SAPO-34 molecular sieve (SP-A), 20g ZSM-5 molecular sieve and 240g deionized water were mixed and stirred for 1h to obtain molecular sieve slurry A; then 59g kaolin, 136g aluminum sol and 85g deionized water were mixed and sheared for 1h to obtain mixed solution B; molecular sieve slurry A and 67g acidified aluminum stone were added to mixed solution B, and sheared for 0.5h to obtain mixed solution C; mixed solution C was spray-dried to prepare a microsphere catalyst, and then the microsphere catalyst was calcined at 500°C for 4h, and then washed with (NH4)2SO4 solution at 60°C until the Na2O content was less than 0.25wt%, followed by rinsing with deionized water and filtering, and then drying at 110°C to obtain a catalytic cracking catalyst, marked as CC sample.

[0075] Catalyst Preparation Example 4

[0076] 60g SAPO-34 molecular sieve (SP-A) was mixed with 180g deionized water and stirred for 1h to obtain molecular sieve slurry A; then 71g kaolin, 100g silica sol and 189g deionized water were mixed and sheared for 1h to obtain mixed solution B; molecular sieve slurry A and 67g aluminum oxide were added to mixed solution B and sheared for 0.5h to obtain mixed solution C; mixed solution C was spray-dried to prepare a microsphere catalyst, and then the microsphere catalyst was calcined at 500°C for 4h, and then washed with (NH4)2SO4 solution at 60°C until the Na2O content was less than 0.25wt%, followed by rinsing with deionized water and filtering, and then drying at 110°C to obtain a catalytic cracking catalyst, marked as CD sample.

[0077] Catalyst Preparation Comparative Example 1

[0078] 60g SAPO-34 molecular sieve (SP-B) was mixed with 180g deionized water and stirred for 1h to obtain molecular sieve slurry A; then 71g kaolin, 182g aluminum sol and 108g deionized water were mixed and sheared for 1h to obtain mixed solution B; molecular sieve slurry A and 67g acidified aluminum stone were added to mixed solution B and sheared for 0.5h to obtain mixed solution C; mixed solution C was spray-dried to prepare a microsphere catalyst, and then the microsphere catalyst was calcined at 500°C for 4h, and then washed with (NH4)2SO4 solution at 60°C until the Na2O content was less than 0.25wt%, followed by rinsing with deionized water and filtering, and then drying at 110°C to obtain a catalytic cracking catalyst, which was marked as a CE sample.

[0079] Catalyst Preparation Comparative Example 2

[0080] 60g ZSM-5 molecular sieve was mixed with 180g deionized water and stirred for 1h to obtain molecular sieve slurry A; then 71g kaolin, 182g aluminum sol and 108g deionized water were mixed and sheared for 1h to obtain mixed solution B; molecular sieve slurry A and 67g acidified aluminum stone were added to mixed solution B and sheared for 0.5h to obtain mixed solution C; mixed solution C was spray-dried to prepare a microsphere catalyst, and then the microsphere catalyst was calcined at 500°C for 4h, and then washed with (NH4)2SO4 solution at 60°C until the Na2O content was less than 0.25wt%, followed by rinsing with deionized water and filtering, and then drying at 110°C to obtain a catalytic cracking catalyst, marked as CF sample.

[0081] Catalyst Preparation Example 5

[0082] 60g SAPO-34 molecular sieve (SP-C) was mixed with 180g deionized water and stirred for 1h to obtain molecular sieve slurry A; then 71g kaolin, 182g aluminum sol and 108g deionized water were mixed and sheared for 1h to obtain mixed solution B; molecular sieve slurry A and 67g acidified aluminum stone were added to mixed solution B and sheared for 0.5h to obtain mixed solution C; mixed solution C was spray-dried to prepare a microsphere catalyst, and then the microsphere catalyst was calcined at 500°C for 4h, and then washed with (NH4)2SO4 solution at 60°C until the Na2O content was less than 0.25wt%, followed by rinsing with deionized water and filtering, and then drying at 110°C to obtain a catalytic cracking catalyst, marked as CG sample.

[0083] Table 1 Dry basis catalyst ingredient ratio (weight %)

[0084]

[0085] Table 2 Characterization of catalyst pore properties

[0086]

[0087] Table 4 Naphtha properties

[0088]

[0089] We aged the six samples obtained in Examples 1-4 and Comparative Examples 1-2 in a fixed bed aging device at 800°C and 100% by volume steam for 17 hours. The aged samples were then evaluated in an ACE Model AP fixed fluidized bed device, using Yanshan Changding naphtha as the raw material, a reaction temperature of 600°C, a catalyst loading of 9g, a catalyst-to-oil ratio of 10 by weight, and a weight hourly space velocity of 4h -1 The gaseous product was analyzed online for composition, and the liquid product was analyzed by simulated distillation. The results are shown in Table 5.

[0090] Table 5 Product selectivity

[0091]

[0092] Product selectivity = product yield (weight) / mass of naphtha converted (weight) × 100%

[0093] It can be seen from the evaluation results in Table 5 that the catalytic cracking catalyst containing lamellar mesoporous SAPO-34 molecular sieve prepared by the present invention has significantly improved selectivity for ethylene and butene in the product compared with the catalyst in the comparative example. Preferably, in the case of containing mesoporous lamellar SAPO-34 molecular sieve, the selectivity for total light olefins (ethylene + propylene + butene) is significantly improved.

Claims

1. A catalytic cracking catalyst containing SAPO-34 molecular sieve, which comprises, based on the total weight of the catalytic cracking catalyst on a dry basis, 1wt% to 80wt% of SAPO-34 molecular sieve, 0wt% to 50wt% of ZSM-5 molecular sieve, 1wt% to 50wt% of binder I, 1wt% to 60wt% of binder II and 1wt% to 40wt% of clay; the SAPO-34 molecular sieve has nano-scale lamellar grains.

2. The catalytic cracking catalyst according to claim 1, characterized in that The mesopore volume of the SAPO-34 molecular sieve accounts for more than 10% of the total pore volume.

3. The catalytic cracking catalyst according to claim 1, characterized in that The molar composition of the SAPO-34 molecular sieve is: 1.0Al2O3: (0.8-1.2)P2O5: (0.2-1.2)SiO2.

4. The catalytic cracking catalyst according to claim 1, characterized in that The SAPO-34 molecular sieve crystal grain thickness does not exceed 200 nm, for example, 20-200 nm, and the crystal grain size is less than 1 micron, for example, 90-980 nm.

5. The catalytic cracking catalyst according to claim 1 or 2, characterized in that: The synthesis method of the SAPO-34 molecular sieve comprises the following steps: (1) mixing an aluminum source, a template agent I and water, stirring for 0 to 30 minutes, then adding a template agent II, and mixing evenly to obtain a mixed solution A; The molar ratio of template I to template II is 0.25 to 4:1, and the molar ratio of the total amount of template I and template II to the aluminum source calculated as Al2O3 is 1 to 4:1; the template I is a template having the function of forming a CHA cage and filling a microporous structure, and the template II is a template that is easily adsorbed on the crystal surface of the grain and has the function of inhibiting the growth of the crystal surface; (2) adding a phosphorus source to the mixed solution A and stirring the mixture to obtain a mixed solution B; (3) Adding a silicon source to the mixed solution B and stirring evenly to obtain a mixed solution C; (4) hydrothermal dynamic crystallization of the mixed solution C at 150-220° C. for 12-120 h; (5) separating, washing, and drying to obtain a solid product; (6) Calcination 6. The catalytic cracking catalyst according to claim 5, characterized in that The silicon source is selected from one or more of silica sol, silicon dioxide, white carbon black or tetraethyl orthosilicate; the aluminum source is selected from one or more of boehmite, pseudo-boehmite, alumina, aluminum hydroxide or aluminum isopropoxide; the phosphorus source is one or more of phosphoric acid, phosphorous acid, ammonium dihydrogen phosphate or diammonium hydrogen phosphate; the template agent I is selected from one or more of tetraethylammonium hydroxide, tetraethylammonium chloride or tetraethylammonium bromide; the template agent II is selected from one or more of diethylamine, triethylamine, morpholine or isopropylamine.

7. The catalytic cracking catalyst according to claim 1 or 2, characterized in that: Mixture C has the following molar ratios: SiO2:Al2O3=0.2~1.2; P2O5:Al2O3=0.8~1.2; Template I:Al2O3=0.2~1.8; Template II: Al2O3=0.2~1.8; H2O: Al2O3=20~100.

8. A method for preparing a catalytic cracking catalyst, comprising the following steps: a) mixing SAPO-34 molecular sieve with water to obtain molecular sieve slurry A; b) mixing clay, binder I and water to obtain a mixed solution B; c) mixing the mixed solution B, the molecular sieve slurry A and the binder II to obtain a mixed solution C; d) spray drying the mixed solution C to prepare a microsphere catalyst; and post-treating the microsphere catalyst to obtain a catalytic cracking catalyst.

9. The method for preparing a catalytic cracking catalyst according to claim 8, characterized in that: The binder I is selected from one or more of aluminum sol, silica sol, phosphate aluminum colloid or silica aluminum sol; the binder II is selected from one or more of pseudo-boehmite or acidified pseudo-boehmite; the clay is selected from one or more of kaolin such as halloysite, montmorillonite or diatomaceous earth.

10. A method for catalytic cracking of naphtha, comprising the step of contacting and reacting naphtha with the catalytic cracking catalyst according to any one of claims 1 to 8.