Cold rolling process of austenitic stainless steel 2B material for high-quality surface decoration

Through the cold rolling process of austenitic stainless steel 2B material, including annealing pickling, pre-rolling, chrome steel wire pickling and cold annealing pickling, the surface defects of austenitic stainless steel are solved, and high-quality surface treatment is achieved. It is suitable for In the high-end decoration field, the cost of grinding and polishing is reduced.

CN118926309AActive Publication Date: 2024-11-12GANSU JIU STEEL GRP HONGXING IRON & STEEL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411213243.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-12
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

The surface of austenitic stainless steel 2B is prone to defects such as white spots and highlights after being ground and polished, which makes it impossible to be suitable for high-end surface decoration fields. The conventional pickling process leads to large surface roughness, which increases the cost of grinding and polishing.

Method used

The cold rolling process of austenitic stainless steel 2B material for high-quality surface decoration includes black coil heat treatment line annealing and pickling, 20-roll mill pre-rolling, chromium steel wire pickling, 20-roll mill rolling, cold annealing and pickling and Online leveling treatment can improve the surface brightness and hardness by controlling parameters such as rolling pressure rate, annealing temperature, pickling concentration and electrolytic pickling current.

Benefits of technology

It effectively avoids instability and oxidation of the material surface, reduces surface roughness, improves surface hardness and brightness, and reduces the cost of subsequent grinding and polishing. It is suitable for high-end decoration purposes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118926309A_ABST
    Figure CN118926309A_ABST
Patent Text Reader

Abstract

The invention discloses a cold rolling process for a high-quality austenitic stainless steel 2B material for surface decoration, and relates to the technical field of stainless steel surface treatment. Reasonable heat treatment temperature is selected for the hot-rolled black coil to modify the surface scale of the austenitic stainless steel, grains are refined to increase the surface hardness of the steel coil, and then after the steel coil is rolled to a certain thickness by a cold rolling mill, chromium steel wire pickling treatment is directly adopted without annealing; the surface defects of the raw materials are further removed to achieve surface quality homogenization, then cold rolling is directly carried out to achieve the target thickness, finally, reasonable heat treatment and electrolytic pickling processes are adopted, and flattening treatment is carried out through an online flattening machine, so that the 2B product with the high-quality surface requirement is produced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of stainless steel surface treatment, in particular to a cold rolling process of austenitic stainless steel 2B material for high-quality surface decoration. Background Art

[0002] Conventional austenitic stainless steel is annealed at high temperature, and then pickled with neutral salt electrolysis and medium-high concentration mixed acid (mixed acid of nitric acid and hydrofluoric acid) for better results. However, the medium-high concentration mixed acid pickling removes the Cr-poor area at the grain boundary of austenitic stainless steel and the Cr-poor layer at the interface between the matrix and the oxide scale, resulting in a large surface roughness and the appearance of intergranular corrosion gullies. Due to the roughness of the surface, the light is diffusely reflected, making the surface of austenitic stainless steel observed by the human eye appear white as a whole. At present, the austenitic stainless steel for high-end decoration is mainly 304, 316L, and 904L, which need to be ground and polished. However, the existence of intergranular corrosion gullies on the surface of conventional austenitic stainless steel 2B increases the cost of grinding and polishing. Summary of the invention

[0003] In view of the above technical problems, the present invention provides a cold rolling process for high-quality austenitic stainless steel 2B material for surface decoration, which is used to solve the problem that austenitic stainless steel 2B raw materials are prone to white spots, bright spots and other defects on the surface after grinding and polishing, and cannot be applied to the field of high-end surface decoration.

[0004] In order to achieve the above object, the technical solution of the present invention is as follows: A cold rolling process for high-quality surface decorative austenitic stainless steel 2B material, comprising the following steps: S1. Annealing and pickling of black coil heat treatment line: austenitic hot-rolled black coils with a thickness of 4.5-5.5 mm are rolled on a six-roll mill, with the rolling reduction rate controlled between 10% and 15%. After rolling, annealing is performed, and after annealing, a continuous pickling process of descaling-shot blasting-sulfuric acid pre-pickling-mixed acid pickling is used for pickling; S2, 20-roll mill pre-rolling: using a 20-roll mill to pre-roll the steel coil treated in step S1 to an intermediate thickness of 2.0 mm to 3.5 mm, with the rolling reduction rate controlled at 25% to 60%, to obtain a pre-rolled hardened steel coil; S3, chrome steel wire pickling treatment: the steel coil treated in step S2 is first subjected to degreasing and oil removal treatment, and then the chrome steel wire surface treatment is performed; S4, 20-roll mill rolling: the steel coil processed in step S3 is finally rolled to a final thickness of 0.8 mm to 2.0 mm, and the rolling reduction rate is controlled at 25% to 60%; S5, cold annealing and pickling treatment: the rolled hardened steel coil after the treatment in step S4 is first degreased, then annealed, and then subjected to neutral salt electrolytic pickling treatment; S6, online flattening treatment: flattening the steel coil after the treatment in step S5, and finally obtaining a high-quality decorative austenitic stainless steel 2B surface material; S7, ETD slitting processing: the materials produced in the previous process are processed into fixed length, width and weight according to customer requirements, and the processed materials are packaged and stored.

[0005] Furthermore, in the step S1, the annealing process adopts a furnace temperature control mode, the furnace temperature is set between 1020°C and 1050°C in the whole area, the TV value is 160-180 mm•m / min, the scale breaker adopts an extension mode in the continuous pickling process, and the elongation rate reaches between 1% and 1.5%; the shot blasting adopts a full-cast shot with a diameter of 0.5-0.8 mm, the blasting speed is controlled at 45-54 m / s, and the flow rate is controlled at 8-12 kg / m 2 ; The 2 groups of heavy brushing and dephosphorization gears of sulfuric acid pre-pickling are controlled at gears 5 to 7; the mixed acid concentration of mixed acid pickling is controlled at 120 to 130 g / l of nitric acid, 25 to 30 g / l of hydrofluoric acid, and the acid temperature is controlled at 45 to 50 °C.

[0006] Furthermore, the rolling rollers in step S2 are M42 high-speed steel rollers, the first rolling speed limit is 120-150 m / min, the last rolling speed limit is 80-120 m / min, and the remaining rolling speed limits are unlimited, and the rolling oil flow rate is controlled at 2500-3500 L / min.

[0007] Furthermore, in the step S3, the elongation of the chrome steel wire surface treatment descaling machine is set to between 1.5% and 2%, and two groups of shot blasting machines are used, both of which are cast shots with a diameter of 400 to 600 μm. The current of the shot blasting machine is set to 100 to 110 A, the frequency is set to 35 to 40 Hz, and the process speed is 25 to 30 m / min; the sulfuric acid pickling concentration is adjusted to 250 to 280 g / l, and the acid temperature is controlled at 78 to 82°C; the nitric acid concentration of the mixed acid pickling is 60 to 70 g / l, the hydrofluoric acid concentration is 8 to 10 g / l, and the acid temperature is controlled at 45 to 50°C.

[0008] Furthermore, the rolling rollers in step S4 are M42 high-speed steel rollers, the first rolling speed limit is 120-150 m / min, the last rolling speed limit is 80-120 m / min, and the rolling oil flow rate is controlled at 2500-3500 L / min.

[0009] Furthermore, in the step S5, the conductivity of the degreasing section of the degreasing treatment is controlled at 4-8mS, and the temperature is controlled at 70-75°C; the annealing temperature of the annealing treatment is controlled at 1020°C-1050°C, the furnace pressure is controlled at 8-12Pa, the residual oxygen is controlled at 2%-4%, and the TV value is controlled at 110-120mm·m / min; the current of the pickling treatment is controlled at 4000-6000A, the neutral salt concentration is controlled at 180-200g / l, and the temperature is controlled at 58-62°C; the current of the nitric acid electrolytic pickling is controlled at 1500-2000A, the concentration is controlled at 150-180g / l, and the temperature is controlled at 48-52°C.

[0010] Furthermore, in step S6, the rolling force of the leveler is controlled at 1800-2000 KN, the tension is controlled at 220-250 KN, and the bending roll force is controlled at 20%-30%.

[0011] Compared with the prior art, the present invention has the following beneficial effects: 1. Low-temperature annealing treatment of black coils can effectively avoid unstable oxidation on the surface of the material, thereby modifying the surface oxide scale and improving the surface hardness of the material; pre-rolling on a six-roll mill and low-speed shot blasting treatment can effectively reduce the surface roughness of the material.

[0012] 2. Use a 20-roll mill for pre-rolling, roll the material to an intermediate thickness, and then use chrome steel wire pickling treatment to further increase the surface corrosion depth, which can effectively further treat the difficult-to-remove defects such as surface segregation and pits caused by steelmaking continuous casting and hot rolling, and obtain the final rolling raw material of the rolling mill with better surface quality.

[0013] 3. The low-temperature annealing treatment in the cold treatment line can reduce the hardness of the final product. At the same time, the pure electrolytic pickling process can avoid severe intergranular corrosion on the surface of austenitic stainless steel, making the surface of the material after final online leveling brighter, which provides great advantages for reducing the cost of subsequent grinding and polishing treatment. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 This is the surface micromorphology of conventional process austenitic stainless steel 2B; Figure 2 The surface micromorphology of austenitic stainless steel 2B after treatment by the present invention; Figure 3 This is the surface macro morphology of austenitic stainless steel 2B after conventional process treatment; Figure 4 The macroscopic morphology of the surface of austenitic stainless steel 2B after being treated by the present invention. DETAILED DESCRIPTION

[0015] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present invention. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.

[0016] Embodiment 1, A cold rolling production process of austenitic stainless steel 2B material for high-quality surface decoration, the specific process includes the following steps: S1. Annealing and pickling of black coil heat treatment line: The austenitic hot-rolled black coil with a thickness of 4.5mm is rolled on a six-roll mill, and the rolling reduction rate is controlled at 10%. After rolling, annealing is carried out. The annealing process adopts the furnace temperature control mode. The furnace temperature in the whole area is set at 1020℃, and the TV value is 160mm•m / min. After annealing, the continuous pickling process of descaling-shot blasting-sulfuric acid pre-pickling-mixed acid pickling is adopted for pickling. The descaling machine adopts the extension mode, and the elongation rate reaches 1%. The shot blasting adopts 0.6mm diameter full-cast shot treatment, the throwing speed is controlled at 45m / s, and the flow rate is controlled at 8kg / m 2 , the 2 groups of heavy brushing and dephosphorization gears of sulfuric acid pre-pickling are controlled at gear 5, the mixed acid concentration of mixed acid pickling is controlled at 120g / l nitric acid, 25g / l hydrofluoric acid, and the acid temperature is controlled at 45°C; S2, 20-roll mill pre-rolling: Use a 20-roll mill to pre-roll the steel coil treated in step S1 to an intermediate thickness of 2.0 mm, use M42 high-speed steel rolls, control the rolling reduction rate at 30%, limit the first rolling speed to 120 m / min, limit the last rolling speed to 80 m / min, and the remaining rolling speeds are unlimited, and control the rolling oil flow rate at 2500 L / min to obtain a pre-rolled hardened steel coil; S3, chrome steel wire pickling treatment: the steel coil treated in step S2 is first degreased and deoiled, and then the chrome steel wire surface treatment is performed, the elongation of the chrome steel wire surface treatment scale breaking machine is set to 1.5%, 2 groups of shot blasting machines are used, both of which have a diameter of 400 μm, the shot blasting machine current is set to 100A, the frequency is set to 35HZ, the process speed is 25m / min, the sulfuric acid pickling concentration is adjusted to 250g / l, the acid temperature is controlled at 78°C, the mixed acid pickling nitric acid concentration is 60g / l, the hydrofluoric acid concentration is 8g / l, and the acid temperature is controlled at 45°C; S4, 20-roll mill rolling: the steel coil processed in step S3 is finally rolled, the rolling rolls are selected from M42 high-speed steel rolling rolls, and the final thickness is 0.8 mm. The rolling reduction rate is controlled at 25%, the first rolling speed limit is 120 m / min, the last rolling speed limit is 80 m / min, and the rolling oil flow rate is controlled at 2500 L / min; S5, cold annealing pickling treatment: the rolled hard steel coil after step S4 is first degreased, the conductivity of the degreasing section is controlled at 4mS, the temperature is controlled at 70°C, and annealing is performed after degreasing, the annealing temperature of the annealing treatment is controlled at 1020°C, the furnace pressure is controlled at 8Pa, the residual oxygen is controlled at 2%, and the TV value is controlled at 110mm·m / min. After annealing, neutral salt electrolytic pickling treatment is performed, the current of the pickling treatment is controlled at 4000A, the neutral salt concentration is controlled at 180g / l, and the temperature is controlled at 58°C; the current of nitric acid electrolytic pickling is controlled at 1500A, the concentration is controlled at 150g / l, and the temperature is controlled at 48°C; S6, online leveling treatment: the steel coil treated in step S5 is leveled, the rolling force of the leveling mill is controlled at 1800KN, the tension is controlled at 220KN, and the bending roll force is controlled at 20%, and finally a high-quality decorative austenitic stainless steel 2B surface material is obtained; S7, ETD slitting processing: the materials produced in the previous process are processed into fixed length, width and weight according to customer requirements, and the processed materials are packaged and stored.

[0017] Embodiment 2, A cold rolling production process of austenitic stainless steel 2B material for high-quality surface decoration, the specific process includes the following steps: S1. Annealing and pickling of black coil heat treatment line: The austenitic hot-rolled black coil with a thickness of 5.0 mm is rolled on a six-roll mill, and the rolling reduction rate is controlled at 13%. After rolling, annealing is carried out. The annealing process adopts the furnace temperature control mode. The furnace temperature is set at 1035℃ in the whole area, and the TV value is 170mm•m / min. After annealing, the continuous pickling process of descaling-shot blasting-sulfuric acid pre-pickling-mixed acid pickling is adopted for pickling. The descaling machine adopts the extension mode, and the elongation rate reaches 1.3%. The shot blasting adopts 0.7mm diameter full-cast shot treatment, the throwing speed is controlled at 50m / s, and the flow rate is controlled at 10kg / m 2 , the 2 groups of heavy brushing and dephosphorization gears of sulfuric acid pre-pickling are controlled at gear 6, the mixed acid concentration of mixed acid pickling is controlled at 125g / l nitric acid, 27g / l hydrofluoric acid, and the acid temperature is controlled at 48°C; S2, 20-roll mill pre-rolling: Use a 20-roll mill to pre-roll the steel coil treated in step S1 to an intermediate thickness of 2.8 mm, use M42 high-speed steel rolls, control the rolling reduction rate at 42%, limit the first rolling speed to 135 m / min, limit the last rolling speed to 100 m / min, and the remaining rolling speeds are unlimited, and control the rolling oil flow rate at 3000 L / min to obtain a pre-rolled hardened steel coil; S3, chrome steel wire pickling treatment: the steel coil treated in step S2 is first degreased and deoiled, and then the chrome steel wire surface treatment is performed, the elongation of the chrome steel wire surface treatment scale breaking machine is set to between 1.7%, 2 groups of shot blasting machines are used, both of which have a diameter of 500 μm, the shot blasting machine current is set to 105A, the frequency is set to 38HZ, the process speed is 27m / min, the sulfuric acid pickling concentration is adjusted to 265g / l, the acid temperature is controlled at 80°C, the mixed acid pickling nitric acid concentration is 65g / l, the hydrofluoric acid concentration is 9g / l, and the acid temperature is controlled at 48°C; S4, 20-roll mill rolling: the steel coil processed in step S3 is finally rolled, the rolling rolls are selected from M42 high-speed steel rolling rolls, and the final thickness is 1.4 mm. The rolling reduction rate is controlled at 42%, the first rolling speed limit is 135 m / min, the last rolling speed limit is 100 m / min, and the rolling oil flow rate is controlled at 3000 L / min; S5, cold annealing pickling treatment: the rolled hard steel coil after step S4 is first degreased, the conductivity of the degreasing section is controlled at 6mS, the temperature is controlled at 72°C, and annealing is performed after degreasing, the annealing temperature of the annealing treatment is controlled at 1035°C, the furnace pressure is controlled at 10Pa, the residual oxygen is controlled at 3%, and the TV value is controlled at 115mm·m / min. After annealing, neutral salt electrolytic pickling treatment is performed, the current of the pickling treatment is controlled at 5000A, the neutral salt concentration is controlled at 190g / l, and the temperature is controlled at 60°C; the current of nitric acid electrolytic pickling is controlled at 1750A, the concentration is controlled at 165g / l, and the temperature is controlled at 50°C; S6, online leveling treatment: the steel coil treated in step S5 is leveled, the rolling force of the leveling mill is controlled at 1900KN, the tension is controlled at 235KN, and the bending roll force is controlled at 25%, and finally a high-quality decorative austenitic stainless steel 2B surface material is obtained; S7, ETD slitting processing: the materials produced in the previous process are processed into fixed length, width and weight according to customer requirements, and the processed materials are packaged and stored.

[0018] Embodiment 3, S1. Annealing and pickling of black coil heat treatment line: The austenitic hot-rolled black coil with a thickness of 5.5mm is rolled by a six-roll mill, and the rolling reduction rate is controlled at 15%. After rolling, annealing is carried out. The annealing process adopts the furnace temperature control mode. The furnace temperature is set between 1050℃ in the whole area, and the TV value is 180mm•m / min. After annealing, the continuous pickling process of descaling-shot blasting-sulfuric acid pre-pickling-mixed acid pickling is adopted for pickling. The descaling machine adopts the extension mode, and the elongation rate reaches 1.5%. The shot blasting adopts 0.8mm diameter full-cast shot treatment, the throwing speed is controlled at 54m / s, and the flow rate is controlled at 12kg / m 2, the 2 groups of heavy brushing and dephosphorization gears of sulfuric acid pre-pickling are controlled at gear 7, the mixed acid concentration of mixed acid pickling is controlled at 130g / l nitric acid, 30g / l hydrofluoric acid, and the acid temperature is controlled at 50℃; S2, 20-roll mill pre-rolling: Use a 20-roll mill to pre-roll the steel coil treated in step S1 to an intermediate thickness of 3.5 mm, use M42 high-speed steel rolls, control the rolling reduction rate at 60%, limit the first rolling speed at 150 m / min, limit the last rolling speed at 120 m / min, and the remaining rolling speeds at no speed limit, and control the rolling oil flow at 3500 L / min to obtain a pre-rolled hardened steel coil; S3, chrome steel wire pickling treatment: the steel coil treated in step S2 is first degreased and deoiled, and then the chrome steel wire surface treatment is performed, the elongation of the chrome steel wire surface treatment scale breaking machine is set to 2%, 2 sets of shot blasting machines are used, both of which have a diameter of 600 μm, the shot blasting machine current is set to 110A, the frequency is set to 40HZ, the process speed is 30m / min, the sulfuric acid pickling concentration is adjusted to 280g / l, the acid temperature is controlled at 82°C, the mixed acid pickling nitric acid concentration is 70g / l, the hydrofluoric acid concentration is 10g / l, and the acid temperature is controlled at 50°C; S4, 20-roll mill rolling: the steel coil processed in step S3 is finally rolled, the rolling rolls are selected from M42 high-speed steel rolling rolls, and the final thickness is rolled to 2.0 mm, the rolling reduction rate is controlled at 60%, the first rolling speed limit is 150 m / min, the last rolling speed limit is 120 m / min, and the rolling oil flow rate is controlled at 3500 L / min; S5, cold annealing pickling treatment: the rolled hard steel coil after step S4 is first degreased, the conductivity of the degreasing section is controlled at 8mS, the temperature is controlled at 75°C, and annealing is performed after degreasing, the annealing temperature of the annealing treatment is controlled at 1050°C, the furnace pressure is controlled at 12Pa, the residual oxygen is controlled at 4%, and the TV value is controlled at 120mm·m / min. After annealing, neutral salt electrolytic pickling treatment is performed, the current of the pickling treatment is controlled at 6000A, the neutral salt concentration is controlled at 200g / l, and the temperature is controlled at 62°C; the current of nitric acid electrolytic pickling is controlled at 2000A, the concentration is controlled at 180g / l, and the temperature is controlled at 52°C; S6, online leveling treatment: the steel coil treated in step S5 is leveled, the rolling force of the leveling mill is controlled at 2000KN, the tension is controlled at 250KN, and the bending roll force is controlled at 30%, and finally a high-quality decorative austenitic stainless steel 2B surface material is obtained; S7, ETD slitting processing: the materials produced in the previous process are processed into fixed length, width and weight according to customer requirements, and the processed materials are packaged and stored.

[0019] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A cold rolling process for high-quality surface decorative austenitic stainless steel 2B material, characterized by: The following steps are involved: S1. Annealing and pickling of black coil heat treatment line: austenitic hot-rolled black coils with a thickness of 4.5-5.5 mm are rolled on a six-roll mill, with the rolling reduction rate controlled between 10% and 15%. After rolling, annealing is performed, and after annealing, a continuous pickling process of descaling-shot blasting-sulfuric acid pre-pickling-mixed acid pickling is used for pickling; S2, 20-roll mill pre-rolling: using a 20-roll mill to pre-roll the steel coil treated in step S1 to an intermediate thickness of 2.0 mm to 3.5 mm, with the rolling reduction rate controlled at 25% to 60%, to obtain a pre-rolled hardened steel coil; S3, chrome steel wire pickling treatment: the steel coil treated in step S2 is first subjected to degreasing and deoiling treatment, and then the chrome steel wire surface treatment is performed; S4, 20-roll mill rolling: the steel coil processed in step S3 is finally rolled to a final thickness of 0.8 mm to 2.0 mm, and the rolling reduction rate is controlled at 25% to 60%; S5, cold annealing and pickling treatment: the rolled hardened steel coil after the treatment in step S4 is first degreased, then annealed, and then subjected to neutral salt electrolytic pickling treatment; S6, online flattening treatment: flattening the steel coil after the treatment in step S5, and finally obtaining a high-quality decorative austenitic stainless steel 2B surface material; S7, ETD slitting processing: the materials produced in the previous process are processed into fixed length, width and weight according to customer requirements, and the processed materials are packaged and stored.

2. The cold rolling process of austenitic stainless steel 2B material for high-quality surface decoration according to claim 1 is characterized by: In the step S1, the annealing process adopts the furnace temperature control mode, the furnace temperature is set between 1020℃ and 1050℃, the TV value is 160-180mm•m / min, the scale breaker adopts the extension mode in the continuous pickling process, and the elongation rate reaches between 1% and 1.5%; the shot blasting adopts the full-cast shot with a diameter of 0.5-0.8mm, the blasting speed is controlled at 45-54m / s, and the flow rate is controlled at 8-12kg / m 2 ; The 2 groups of heavy brushing and dephosphorization gears of sulfuric acid pre-pickling are controlled at gears 5 to 7; the mixed acid concentration of mixed acid pickling is controlled at 120 to 130 g / l of nitric acid, 25 to 30 g / l of hydrofluoric acid, and the acid temperature is controlled at 45 to 50 °C.

3. The cold rolling process of austenitic stainless steel 2B material for high-quality surface decoration according to claim 2, characterized in that: The rolling rollers in step S2 are M42 high-speed steel rollers, the first rolling speed limit is 120-150 m / min, the last rolling speed limit is 80-120 m / min, and the remaining rolling speed limits are unlimited. The rolling oil flow rate is controlled at 2500-3500 L / min.

4. The cold rolling process of austenitic stainless steel 2B material for high-quality surface decoration according to claim 3 is characterized by: In the step S3, the elongation of the chrome steel wire surface treatment descaling machine is set to between 1.5% and 2%, and two groups of shot blasting machines are used, both of which have cast shots with a diameter of 400 to 600 μm. The current of the shot blasting machine is set to 100 to 110 A, the frequency is set to 35 to 40 Hz, and the process speed is 25 to 30 m / min; the sulfuric acid pickling concentration is adjusted to 250 to 280 g / l, and the acid temperature is controlled at 78 to 82°C; the nitric acid concentration of the mixed acid pickling is 60 to 70 g / l, the hydrofluoric acid concentration is 8 to 10 g / l, and the acid temperature is controlled at 45 to 50°C.

5. The cold rolling process of austenitic stainless steel 2B material for high-quality surface decoration according to claim 4, characterized in that: The rolling rollers in step S4 are M42 high-speed steel rollers, the first rolling speed limit is 120-150 m / min, the last rolling speed limit is 80-120 m / min, and the rolling oil flow rate is controlled at 2500-3500 L / min.

6. The cold rolling process of austenitic stainless steel 2B material for high-quality surface decoration according to claim 5, characterized in that: In the step S5, the conductivity of the degreasing section of the degreasing treatment is controlled at 4-8mS, and the temperature is controlled at 70-75°C; the annealing temperature of the annealing treatment is controlled at 1020°C-1050°C, the furnace pressure is controlled at 8-12Pa, the residual oxygen is controlled at 2%-4%, and the TV value is controlled at 110-120mm·m / min; the current of the pickling treatment is controlled at 4000-6000A, the neutral salt concentration is controlled at 180-200g / l, and the temperature is controlled at 58-62°C; the current of the nitric acid electrolytic pickling is controlled at 1500-2000A, the concentration is controlled at 150-180g / l, and the temperature is controlled at 48-52°C.

7. The cold rolling process of austenitic stainless steel 2B material for high-quality surface decoration according to claim 6, characterized in that: In step S6, the rolling force of the leveler is controlled at 1800-2000 KN, the tension is controlled at 220-250 KN, and the bending roll force is controlled at 20%-30%.

Citation Information

Patent Citations

  • Cold rolling process for 304 stainless steel 2B base material for decorative panel

    CN106807751A

  • Manufacturing method of cold-rolled SUS304 two-sided bright-annealed (BA) surface stainless steel

    CN108950159A

  • Cold rolling for 2B surface of 439 ferrite stainless steel

    CN110814032A

  • Manufacturing method of high-performance austenitic stainless steel for surface decoration industry

    CN116926293A

  • Production process of ultra-pure ferritic stainless steel BA coiled material base material for automobile bright exterior trim strip

    CN118122807A