Method for improving plate-plate cementing quality in large-curvature area
By using mold release fabric or pressure-sensitive tape to compensate during the adhesive bonding process of composite material boards, and combining with the adhesive film to compensate for the adhesive gap, the bubble and debonding problems caused by insufficient or excessive film compensation in traditional adhesive bonding are solved. , improves the bonding quality and bonding sufficiency.
Patent Information
- Application Number
- CN202410856091.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During the glue bonding process of traditional composite boards, when the curvature of the adhesive surface is large, the gap between the adhesive interface is large, resulting in insufficient or excessive compensation of the adhesive film, which is prone to bubbles and debonding problems, affecting the quality of the adhesive.
During the bonding process, use a mold release cloth or pressure-sensitive tape to compensate the bonding component and the mold, combine it with the glue film to compensate for the bonding gap, and perform the mold compensation outside the bonding gap to reduce the amount of glue film and interface gap.
It effectively reduces the chance of gas clamping between the adhesive film layers, reduces the interface gap between components, and improves the bonding quality and adhesion sufficiency.
Smart Images

Figure CN118927757A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite material manufacturing process, and relates to a method for improving the quality of plate-to-plate bonding in a large curvature area. Background Art
[0002] Composite materials have many advantages such as high strength, low specific gravity, and good heat resistance. They have developed into one of the most important structural materials for modern commercial aircraft and are widely used in the aerospace field. Composite bonding is the use of polymer materials as adhesives to bond cured composite parts or metal parts to other cured composite parts, honeycomb cores, foam cores or metal parts. Secondary bonding is the bonding of the cured prepreg skin with internal honeycomb cores, ribs, reflectors and other components using adhesive films; board-to-board bonding is the bonding form between composite laminates.
[0003] At present, the traditional board-to-board bonding process includes the steps of component surface treatment - component assembly - component bonding verification and film compensation - curing and demoulding. The film verification is required before the board-to-board bonding is cured. When the curvature of the surface to be bonded is large, the matching relationship between the components to be bonded is poor, which will form a large gap between the bonding interfaces. The traditional film compensation method requires a large amount of film compensation to fill the bonding gap to ensure that the components to be bonded can be bonded; however, this film compensation method has a major drawback. When the amount of film compensation is too much, it is easier for the film layers to trap gas, resulting in bubbles in the cured adhesive layer and the formation of diffuse pores, which will be judged as defects by the inspectors during non-destructive testing; in addition, the film is fluid during the temperature rise and curing process, resulting in the film glue flowing out of the bonding gap during the curing process. The original compensated film is not enough to fill the interface gap, resulting in debonding problems at the bonding interface.
[0004] The traditional film compensation method requires a large amount of film compensation to fill the bonding gap to ensure that the components to be bonded can be bonded; however, this film compensation method has major drawbacks. When the amount of film compensation is too much, it is easier for gas to be trapped between the film layers, causing bubbles to form in the cured adhesive layer, forming diffuse pores, which will be judged as defects by inspectors during non-destructive testing; in addition, the film is fluid during the temperature increase and curing process, causing the film glue to flow out of the bonding gap during the curing process, and the original compensation film is not enough to fill the interface gap, resulting in debonding problems at the bonding interface. Summary of the invention
[0005] Purpose of the Invention
[0006] The method of the present invention is to perform bonding by combining the method of filling the bonding gap with the film compensation and reducing the bonding gap with the method of performing profile compensation outside the bonding gap during the bonding inspection and film compensation of the components. The advantages of the present invention are that the profile compensation outside the bonding interface reduces the amount of the film, reduces the probability of gas being trapped between the film layers, and reduces the interface gap of the components, making it easier for the components to be fully bonded.
[0007] Technical Solution
[0008] A method for improving the quality of board-to-board bonding in areas with large curvature.
[0009] The present invention aims to use a release cloth or a pressure-sensitive tape to compensate between the component to be bonded and the mold when bonding a large curvature profile area of a composite material, thereby reducing the bonding interface gap of the component to be bonded and the amount of adhesive film compensation, and improving the bonding quality. The specific steps are as follows:
[0010] Step 1: Treat the surface of the components to be bonded (such as end ribs and skins) by using 80#~120# sandpaper to roughen the surface of the parts and remove the resin gloss on the surface of the parts; or treat the surface of the parts by sandblasting and use brown corundum abrasive to blow and remove the gloss on the surface of the parts.
[0011] Step 2: Assemble the components to be glued onto the bonding tooling according to the digital model positions, check whether the dimensions between the components meet the requirements, and repair the areas where there is interference between the components.
[0012] Step three, lay a 0.2-0.4mm thick adhesive film on the interface of the component area to be bonded for calibration, and then evenly place calibration wires on the surface of the calibration film with a spacing of 5-20mm. After sealing the vacuum bag, transfer it to the autoclave and apply external pressure to 0.1-0.3MPa for calibration for 30-60min. After the calibration is completed, check whether the calibration wire has pressed out clear and visible marks on the adhesive film. Compensate with the adhesive film in the area where no calibration marks are pressed out and repeat this step until all calibration marks are clearly visible.
[0013] Step 4: After the verification and compensation process is completed, place isolation film, paint cloth, breathable felt and other auxiliary materials on the surface of the component, then use sealing strips to seal the vacuum bag, transfer it to an autoclave or oven for curing, and demold it after curing.
[0014] Furthermore, the calibration wire has a diameter of 0.1 to 0.2 mm.
[0015] Furthermore, the brown corundum abrasive has a particle size of less than 80#.
[0016] Furthermore, the purging is performed no more than 2 times.
[0017] Furthermore, in the area where no verification mark is pressed out, continue to lay 0.2-0.4mm adhesive film;
[0018] Furthermore, in the area where no verification marks are pressed out, the corresponding area is found on the mold surface, and adhesive auxiliary materials such as release cloth and pressure-sensitive tape are used for eccentric compensation. The compensation diagram is shown in Figure 1 As shown;
[0019] Furthermore, the number of compensation layers of auxiliary materials such as release cloth, pressure-sensitive tape and other adhesives is 1 to 10 layers; further, the laying spacing between different layers of auxiliary materials such as release cloth, pressure-sensitive tape and other adhesives is required to be 5 to 10 mm.
[0020] Technical Effects
[0021] When bonding the large curvature profile area of the composite material, the present invention uses a release cloth or a pressure-sensitive tape to compensate between the component to be bonded and the mold, reducing the bonding interface gap of the component to be bonded and the amount of film compensation at the bonding interface. The method of the present invention is to bond by combining film compensation to fill the bonding gap and profile compensation outside the bonding gap to reduce the bonding gap during the bonding inspection and film compensation of the components. The advantage of the present invention is that the profile compensation outside the bonding interface reduces the amount of film, reduces the probability of gas entrapment between film layers, and reduces the interface gap of the components, making it easier for the components to be fully bonded. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 Schematic diagram of the bonding structure location;
[0023] Figure 2 Schematic diagram of the out-of-position compensation position. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical scheme and advantages of the implementation of the present invention clearer, the technical scheme in the embodiment of the present invention will be described in more detail below in conjunction with the drawings in the embodiment of the present invention. In the drawings, the same or similar reference numerals throughout represent the same or similar originals or elements with the same or similar functions. The described embodiments are part of the embodiments of the present invention, not all of the embodiments. The embodiments described below with reference to the drawings are exemplary and intended to be used to explain the present invention, and should not be construed as limitations on the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. The embodiments of the present invention are described in detail below in conjunction with the drawings.
[0025] The present invention aims to use a release cloth or a pressure-sensitive tape to compensate between the component to be bonded and the mold when bonding a large curvature surface area of a composite material, thereby reducing the bonding interface gap of the component to be bonded and the amount of film compensation, and avoiding board-to-board debonding or board-to-board diffusion defects caused by excessive film compensation.
[0026] Step 1: Treat the surface of the components to be bonded (such as end ribs and skins) by blowing the surface of the parts twice with 80# brown corundum abrasive to remove the gloss on the surface of the parts.
[0027] Step 2: Assemble the components to be glued onto the bonding tooling according to the digital model positions, check whether the dimensions between the components meet the requirements, and adjust the matching clearance of the components to less than 1mm.
[0028] Step three, lay a 0.2mm thick adhesive film on the interface of the component area to be bonded for verification, and then evenly place calibration wires with a diameter of about 0.1mm on the surface of the calibration film, with a spacing of 10mm. After sealing the vacuum bag, transfer it to the autoclave and apply external pressure to 0.1MPa for verification for 30 minutes. After the verification is completed, check whether the calibration wire has pressed out clear and visible marks on the adhesive film. In the area where no calibration marks are pressed out, perform adhesive film compensation and repeat this step until all calibration marks are clearly visible.
[0029] In a certain implementation case of the present invention, in the area where no verification mark is pressed out, a 0.2 mm thick film is continuously laid;
[0030] In a certain implementation case of the present invention, in the area where the verification mark is not pressed out, the corresponding area is found on the mold surface, and 5 layers of mold release cloth are used for out-of-position compensation. The compensation schematic diagram is shown as follows: Figure 1 As shown;
[0031] In a certain embodiment of the present invention, the laying spacing between different layers of auxiliary materials such as release cloth, pressure-sensitive tape and other adhesive materials is required to be 10 mm.
[0032] Step 4: After the verification and compensation process is completed, place isolation film, paint cloth, breathable felt and other auxiliary materials on the surface of the component, then use sealing strips to seal the vacuum bag, transfer it to an autoclave or oven for curing, and demold it after curing.
[0033] In a certain implementation case of the present invention, the calibration wire has a diameter of 0.1 to 0.2 mm.
[0034] In a certain embodiment of the present invention, the brown corundum abrasive has a particle size of less than 80#.
[0035] In a certain implementation case of the present invention, the purging is performed no more than 2 times.
[0036] In a certain implementation case of the present invention, in the area where no verification mark is pressed out, a 0.2-0.4 mm thick film is continuously laid;
[0037] In a certain embodiment of the present invention, in the area where the verification mark is not pressed out, the corresponding area is found on the mold surface, and the mold release cloth, pressure-sensitive tape and other adhesive auxiliary materials are used to perform ectopic compensation. The compensation schematic diagram is shown in FIG. Figure 1 As shown;
[0038] In a certain embodiment of the present invention, the number of compensation layers of auxiliary materials such as release cloth, pressure-sensitive tape, etc. that can be adhered is 1 to 10 layers;
[0039] In a certain embodiment of the present invention, the laying spacing between different layers of auxiliary materials such as release cloth, pressure-sensitive tape and other adhesive materials is required to be 5 to 10 mm.
[0040] When bonding the large curvature profile area of the composite material, the present invention uses a release cloth or a pressure-sensitive tape to compensate between the component to be bonded and the mold, reducing the bonding interface gap of the component to be bonded and the amount of film compensation at the bonding interface. The method of the present invention is to bond by combining film compensation to fill the bonding gap and profile compensation outside the bonding gap to reduce the bonding gap during the bonding inspection and film compensation of the components. The advantage of the present invention is that the profile compensation outside the bonding interface reduces the amount of film, reduces the probability of gas entrapment between film layers, and reduces the interface gap of the components, making it easier for the components to be fully bonded.
[0041] It is understood by those skilled in the art that, unless otherwise defined, all terms (including technical terms and scientific terms) used herein have the same meaning as the general understanding of ordinary technicians in the field to which the present invention belongs. It should also be understood that terms such as those defined in general dictionaries should be understood to have the same meaning as in the context of the prior art, and unless defined as here, will not be interpreted with idealized or overly formal meanings. The specific implementation methods described above further describe the purpose, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the present invention. Within the spirit and principle of the present invention, any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment of equivalent changes for application in other fields, but any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the technical solution content of the present invention, any modification, equivalent replacement, improvement, etc., made according to the technical essence of the present invention, should be included in the protection scope of the present invention.
Claims
1. A method for improving the quality of board-to-board bonding in a large curvature area, characterized in that: When bonding large curvature surface areas of composite materials, use release cloth or pressure-sensitive tape to compensate between the components to be bonded and the mold to reduce the bonding interface gap and the amount of film compensation of the components to be bonded. The specific steps are as follows: Step 1: Treat the surface of the components to be bonded by using sandpaper to roughen the surface of the components and remove the resin gloss on the surface of the components; Step 2: Assemble the components to be bonded onto the bonding tooling according to the digital model positions, check whether the dimensions between the components meet the requirements, and repair the areas where the components interfere; Step 3: Lay a 0.2-0.4mm adhesive film on the interface of the component to be bonded for verification, and then evenly place the calibration wire on the surface of the calibration film with a spacing of 5-20mm. After sealing the vacuum bag, transfer it to the autoclave and apply external pressure to 0.1-0.3MPa for verification for 30-60min. After the verification is completed, check whether the calibration wire has pressed out a clear and visible mark on the adhesive film. Compensate the area where the calibration mark is not pressed out with the adhesive film and repeat this step until all the calibration marks are clearly visible. Step 4: After the verification and compensation process is completed, place isolation film, paint cloth, and breathable felt auxiliary materials on the surface of the components, then use sealing strips to seal the vacuum bag, transfer it to an autoclave or oven for curing, and demold it after curing.
2. The method according to claim 1, characterized in that The calibration wire has a diameter of 0.1 mm to 0.2 mm.
3. The method according to claim 2, characterized in that In step 1, the surface treatment is performed by sandblasting the surface of the part, and brown corundum abrasive is used for blowing to remove the gloss on the surface of the part; the brown corundum abrasive is selected to have a particle size of less than 80#.
4. The method according to claim 3, characterized in that Purge no more than 2 times.
5. The method according to claim 4, characterized in that In the area where no verification marks are pressed out, continue to lay 0.2-0.4mm adhesive film.
6. The method according to claim 5, characterized in that In the area where no verification marks are pressed out, find the corresponding area on the mold surface and use release cloth, pressure-sensitive tape or other adhesive auxiliary materials to compensate for the eccentricity.
7. The method according to claim 6, characterized in that The number of compensation layers of release cloth, pressure-sensitive tape and adhesive auxiliary materials is 1 to 10 layers.
8. The method according to claim 7, characterized in that The laying spacing between different layers of release cloth, pressure-sensitive tape and adhesive auxiliary materials is required to be 5mm to 10mm.
9. A large curvature glued plate, characterized in that: A method according to any one of claims 1 to 8 is adopted.
10. A large curvature adhesive bonded plate as claimed in claim 9, characterized in that: Application in composite material manufacturing.
Citation Information
Patent Citations
Conformal antenna structure cementing compensation method
CN115207601A
Verification method for plate-plate structure glue joint between skin and beam frame
CN117549575A
Verification method for composite material plate-plate glue joint
CN117818080A
Composite material honeycomb sandwich verification method
CN118205215A