Coupling thallium removal agent and preparation method thereof

By constructing a coupled thallium removal agent for amorphous polyferrous sulfide active substance on the surface of zeolite powder, the problems of low thallium concentration and high cost in industrial thallium-containing wastewater treatment are solved, and an efficient and economical deep thallium removal effect is achieved.

CN118929773APending Publication Date: 2024-11-12HUNAN ZHUYE ENVIRONMENT TECH CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410949224.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art is difficult to effectively and economically treat industrial thallium-containing wastewater, especially due to the low thallium concentration and large treatment volume, resulting in high cost and poor effect of thallium removal methods.

Method used

Zeolite powder is used as a carrier, combined with amorphous polyferrous sulfide active substances, and combined with zeolite through ferrite bonds and sulfur-oxygen bonds to form a coupled thallium removal agent, and uses its large specific surface area and thallium-philic properties to achieve deep thallium removal.

Benefits of technology

High selectivity and deep thallium removal for industrial thallium-containing wastewater are achieved, reducing the cost of thallium removal, avoiding side reactions and secondary slag production, and improving the utilization rate of sulfur ions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929773A_ABST
    Figure CN118929773A_ABST
Patent Text Reader

Abstract

The invention provides a coupling thallium removal agent. The coupling thallium removal agent comprises zeolite powder serving as a carrier and an amorphous ferrous polysulfide active substance combined on the surface layer of the zeolite powder, wherein the amorphous ferrous polysulfide active substance is combined with the zeolite through an iron-oxygen bond and a sulfur-oxygen bond. The invention further provides a preparation method of the coupling thallium removal agent. The coupling thallium removal agent provided by the invention has relatively high selectivity, and the preparation method of the coupling thallium removal agent provided by the invention has the advantages of low consumption and low cost, and can realize economical and efficient deep removal of thallium from industrial thallium-containing wastewater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wastewater treatment in nonferrous metallurgy, and in particular to a coupled thallium removal agent and a preparation method thereof. Background Art

[0002] Scattered metal thallium is mainly associated with lead, zinc, copper and iron minerals. Thallium-containing wastewater is easily generated during mining, metal smelting and processing. Industrial thallium-containing wastewater has the characteristics of complex composition, low concentration, high toxicity and large treatment volume. Thallium can cause serious harm to the human central nervous system, cardiovascular system and digestive system, and pose a threat to the ecological environment and human health. At present, the discharge standard of thallium-containing wastewater has been reduced to below 5μg / L. Therefore, it is very important to develop effective thallium-containing wastewater treatment technology.

[0003] At present, physical, chemical and biological methods are mainly used to treat industrial thallium-containing wastewater. Among them, physical methods are mainly adsorption, and the main materials are activated carbon, iron-based materials, manganese-based materials, and titanium-based materials. In addition, physical methods also include ion exchange, membrane technology and other thallium removal methods. Chemical methods include precipitation, oxidation, flocculation, electrochemical methods and other methods. Among them, precipitation is mainly sulfide precipitation, which has the characteristics of simple process and low cost and is widely used. Flocculation and electrochemical methods mainly remove thallium by adding iron-based or aluminum-based flocculants to wastewater. In addition, biological methods for thallium removal mainly include microbial fixation and biological adsorption, but there are still problems to be solved in strain design and thallium recovery.

[0004] Although there are many studies on the treatment technology of industrial thallium-containing wastewater, the concentration of thallium in industrial thallium-containing wastewater is usually low, so a thallium removal agent with good selectivity is needed. And because the amount of industrial thallium-containing wastewater is large, the cost of thallium removal from wastewater should be low to improve economic benefits. However, the current methods and principles of thallium removal from wastewater are often relatively simple, and these thallium removal methods have more or less some shortcomings. If we want to remove thallium from industrial thallium-containing wastewater economically, efficiently, simply and deeply, we still face some technical challenges.

[0005] Therefore, there is an urgent need to develop a thallium removal agent with high selectivity and low consumption to achieve economical and efficient deep thallium removal from industrial thallium-containing wastewater. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a coupled thallium removal agent with high selectivity and low consumption and a preparation method thereof, so as to achieve economical and efficient deep thallium removal for industrial thallium-containing wastewater.

[0007] In order to solve the above technical problems, the present invention provides a coupled thallium removal agent, comprising zeolite powder as a carrier and an amorphous ferrous polysulfide active substance combined with the surface of the zeolite powder;

[0008] Wherein, the amorphous ferrous polysulfide active material is bonded to the zeolite via an iron-oxygen bond and a sulfur-oxygen bond;

[0009] The structural formula of the coupled thallium removal agent includes:

[0010]

[0011] Furthermore, the specific surface area of ​​the zeolite powder is 80 to 400 m 2 / g, and the average particle size is 10 to 300 microns.

[0012] Preferably, the specific surface area of ​​the zeolite powder is 200 to 400 m 2 / g.

[0013] The present invention provides a method for preparing a coupled thallium removal agent, comprising the following steps:

[0014] adding malic acid solution to zeolite powder to form a weakly acidic precursor solution;

[0015] Adding ferric sulfate crystals to the precursor solution, stirring and reacting to obtain a ferrous malate complex solution;

[0016] Adding Na2S / Na2S2 mixed crystals to the mixed solution, heating to dissolve and evaporating to crystallize, to obtain a residual solution containing amorphous ferrous polysulfide active material adsorbed on the surface of zeolite powder;

[0017] The residual liquid is separated into solid and liquid to obtain a coupled thallium removal agent.

[0018] Furthermore, the specific surface area of ​​the zeolite powder is 80 to 400 m 2 / g, and the average particle size is 10 to 300 microns.

[0019] Preferably, the specific surface area of ​​the zeolite powder is 200 to 400 m 2 / g.

[0020] Furthermore, the mass of malic acid in the malic acid solution is 3% to 10% of the mass of the zeolite powder, and the mass of solvent water in the malic acid solution is 2.5 to 6 times of the mass of the zeolite powder.

[0021] Preferably, the mass of malic acid in the malic acid solution is 5% to 8% of the mass of the zeolite powder, and the mass of the solvent water in the malic acid solution is 3 to 5 times the mass of the zeolite powder.

[0022] Furthermore, the added amount of the ferric sulfate crystals is 1% to 6% of the mass of the zeolite powder.

[0023] Preferably, the added amount of the ferric sulfate crystals is 2% to 4% of the mass of the zeolite powder.

[0024] Furthermore, the reaction temperature after adding iron sulfate crystals to the precursor solution is 40-80° C., and the reaction time is 0.5-2 h.

[0025] Preferably, the reaction temperature after adding iron sulfate crystals to the precursor solution is 50-60°C.

[0026] Furthermore, the added amount of the Na2S / Na2S2 mixed crystals is 0.6 to 1.3 times the mass of ferric sulfate.

[0027] Furthermore, the mass percentage of Na2S in the Na2S / Na2S2 mixed crystal is 10-50%.

[0028] Preferably, the mass percentage of Na2S in the Na2S / Na2S2 mixed crystals is 30-50%.

[0029] Furthermore, the temperature during the heating and evaporation process is 80-100°C.

[0030] Furthermore, the evaporation rate of the evaporated solution is 50-90%.

[0031] Preferably, the evaporation rate of the evaporated solution is 60-80%.

[0032] The coupled thallium removal agent provided by the present invention takes zeolite powder as a matrix, constructs an amorphous ferrous polysulfide active substance on the surface of the zeolite powder, gives full play to the large specific surface area characteristics of zeolite and the thallium affinity reaction characteristics of the amorphous ferrous polysulfide active substance, achieves a physical-chemical coupled thallium removal effect, can greatly improve the thallium removal effect of thallium-containing industrial wastewater, and realizes the purpose of deep thallium removal.

[0033] In addition, the coupled thallium removal agent provided by the present invention constructs an amorphous ferrous polysulfide active substance on the surface of zeolite powder, and utilizes the natural sulfur- and iron-philic properties of metallic thallium to selectively combine with thallium in thallium-containing wastewater to achieve directional thallium removal, and can deeply remove thallium from thallium-containing wastewater with high selectivity.

[0034] At the same time, the preparation method of the coupled thallium removal agent provided by the present invention greatly reduces the unit price of zeolite as a carrier compared to the current aluminum-based, titanium-based and other adsorption materials. And compared to the traditional sodium sulfide direct precipitation method, since the sulfide ions are fixed by ferrous iron in the present invention, the problem of greatly excessive actual dosage due to the hydrolysis side reaction after sodium sulfide is directly added to the wastewater can be avoided. Moreover, each sulfide ion in the coupled thallium removal agent prepared by the present invention can participate in the direct thallium removal reaction, and no side reaction occurs, which improves the utilization rate of sulfide ions and reduces the production of secondary slag, with obvious comprehensive benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1A flow chart of a method for preparing a coupling thallium removal agent provided in an embodiment of the present invention;

[0036] Figure 2 The XRD pattern of the coupled thallium removal agent prepared by the preparation method of the coupled thallium removal agent provided in Example 1 of the present invention;

[0037] Figure 3 The XPS graph of the coupled thallium removal agent prepared by the preparation method of the coupled thallium removal agent provided in Example 1 of the present invention;

[0038] Figure 4 This is a SEM image of the coupled thallium removal agent prepared by the preparation method of the coupled thallium removal agent provided in Example 1 of the present invention. DETAILED DESCRIPTION

[0039] A coupled thallium removal agent provided in an embodiment of the present invention comprises zeolite powder as a carrier and an amorphous ferrous polysulfide active substance bound to the surface of the zeolite powder. The structural formula of the coupled thallium removal agent provided by the present invention is:

[0040]

[0041] The amorphous ferrous polysulfide active material is combined with aluminum and silicon in the zeolite through iron-oxygen bonds and sulfur-oxygen bonds.

[0042] Among them, the specific surface area of ​​zeolite powder is 80~400m 2 / g, and the average particle size is 10 to 300 microns.

[0043] As a preferred embodiment of the present invention, the specific surface area of ​​the zeolite powder is 200 to 400 m 2 / g.

[0044] A coupled thallium removal agent provided by the present invention, with a porous zeolite of large specific area as a carrier, has a good physical adsorption effect on floccules and tiny particles, and can closely adsorb the synthesized amorphous ferrous polysulfide active material on its surface. In addition, when the coupled thallium removal agent of the present invention is added to thallium-containing industrial wastewater, because thallium has a stronger geochemical sulfur affinity, the ferrous polysulfide in the coupled thallium removal agent encounters a thallium ion with a stronger sulfur affinity, and dissociation and disproportionation reactions will occur to generate insolubles of thallium sulfide and thallium iron sulfide, and the generated thallium sulfide and thallium iron sulfide insolubles are closely combined with the zeolite matrix through the original Fe-O bond and SO bond. And because the zeolite as a carrier has a huge surface area, the overall effect of thallium removal can be further improved.

[0045] Therefore, the coupled thallium removal agent provided by the present invention, the amorphous ferrous polysulfide active substance adsorbed on the surface of the zeolite with a huge surface area undergoes a chemical disproportionation precipitation reaction with the thallium in the industrial wastewater, and through the dual effects of chemical selective precipitation-physical enhanced adsorption, the effect of deep thallium removal from thallium-containing industrial wastewater can be achieved.

[0046] See also Figure 1 The present invention provides a method for preparing a coupled thallium removal agent, comprising the following steps:

[0047] Step 1) Slurry preparation: Add malic acid solution into zeolite powder to form a uniform weakly acidic precursor solution.

[0048] In order to improve the mixing effect and make the reaction more thorough and uniform, the specific surface area of ​​zeolite powder is 80-400m 2 / g, and the average particle size is 10 to 300 microns.

[0049] As a preferred embodiment of the present invention, the specific surface area of ​​the zeolite powder is preferably 200 to 400 m 2 / g.

[0050] Among them, malic acid plays the role of stabilizing pH, reducing trivalent iron and coordinating ferrous iron in the subsequent process. If too little water is used for slurry mixing, the slurry will be viscous, which is not conducive to uniform dispersion. If too much water is used, the solute concentration will be low, which will easily increase the subsequent evaporation. Therefore, the mass of malic acid in the malic acid solution is controlled to be 3% to 10% of the mass of the zeolite powder, and the mass of the solvent water in the malic acid solution is controlled to be 2.5 to 6 times the mass of the zeolite powder.

[0051] As a preferred embodiment of the present invention, the mass of malic acid in the malic acid solution is preferably 5% to 8% of the mass of the zeolite powder, and the mass of the solvent water in the malic acid solution is preferably 3 to 5 times the mass of the zeolite powder.

[0052] Step 2) Reduction and coordination: Add ferric sulfate crystals to the precursor solution, and conduct reduction and coordination reaction under stirring to obtain a coordination solution of ferrous malate, and form a uniform slurry with zeolite powder. The ferrous iron can be adsorbed on the oxygen sites of the zeolite to form active ions in the adsorption layer.

[0053] The present invention selects malic acid as an acidity regulator, a reducing agent and a complexing agent, so that ferric sulfate is reduced to form ferrous ions, and ferrous ions and malate form ferrous complex ions. In addition, the weakly acidic environment of malic acid can ensure that ferrous ions are not hydrolyzed, and a stable precursor complexing liquid is formed with zeolite in the form of complex ions. At the same time, after ferrous complexation, it is ensured that its sulfurization reaction will not be completed quickly in the subsequent sulfurization transformation process, and amorphous precipitation can be uniformly formed on the zeolite surface in the stirred solution, without causing local segregation, and the surface area utilization rate of zeolite can be improved.

[0054] The added amount of ferric sulfate crystals is 1% to 6% of the mass of the zeolite powder.

[0055] As a preferred embodiment of the present invention, the amount of ferric sulfate crystals added is preferably 2% to 4% of the mass of the zeolite powder.

[0056] The temperature at which the iron sulfate crystals undergo reduction and complexing reactions in the precursor solution is 40 to 80° C., and the reaction time is 0.5 to 2 hours.

[0057] As a preferred embodiment of the present invention, the temperature at which the ferric sulfate crystals undergo reduction and complexing reactions in the precursor solution is preferably 50-60°C.

[0058] Step 3) Sulfurization evaporation: Add Na2S / Na2S2 mixed crystals to the obtained ferrous malate complex solution, heat to dissolve and evaporate to crystallize, and obtain a residual solution containing amorphous ferrous polysulfide active material adsorbed on the surface of zeolite powder. Among them, ferrous malate complex ions and Na2S / Na2S2 roots undergo sulfidation transformation, and amorphous ferrous polysulfide active material is obtained in a weakly acidic environment and adsorbed on the surface of zeolite.

[0059] The added amount of Na2S / Na2S2 mixed crystals is 0.6 to 1.3 times the mass of ferric sulfate.

[0060] Among them, in the mixed crystal of Na2S / Na2S2, if the mass percentage of Na2S is too low, the sulfur content in the generated ferrous polysulfide is small, and the amount of combined thallium will be small; on the contrary, if the mass percentage of Na2S is too high, it is not conducive to the generation of amorphous ferrous sulfide, and the reaction activity of ferrous polysulfide will be reduced. Therefore, the mass percentage of Na2S in the Na2S / Na2S2 mixed crystal is controlled to be 10-50%.

[0061] As a preferred specific embodiment of the present invention, the mass percentage of Na2S in the Na2S / Na2S2 mixed crystals is preferably 30-50%.

[0062] Among them, in the process of heating and evaporating the ferrous malate complex solution with Na2S / Na2S2 mixed crystals added, in order to facilitate the dissolution of Na2S / Na2S2 and the evaporation of water in the complex solution and promote the formation of amorphous ferrous polysulfide adsorbed on the surface of zeolite powder, the heating evaporation temperature is controlled at 80-100°C.

[0063] At the same time, in order to ensure the stability of the amorphous ferrous polysulfide active material adsorbed on the surface of the zeolite powder in the complex liquid, the complex liquid is not evaporated to dryness during evaporation and crystallization, but a certain amount of water is left to form a residual liquid. The water evaporation rate of the complex liquid is controlled to be 50-90% during evaporation.

[0064] As a preferred embodiment of the present invention, the evaporation rate of the water-evaporated solution is preferably 60 to 80%.

[0065] By adding Na2S / Na2S2, the two sulfur ions react with the ferrous iron in ferrous malate to generate ferrous polysulfide FeSx. Since the reaction is carried out in a low temperature and uniform solution environment, the generated ferrous polysulfide FeSx has an amorphous, highly dispersed and homogeneous form.

[0066] Wherein, the reactions occurring in the process of step 2) and step 3) are as follows:

[0067]

[0068] Step 4) separating the residual liquid from the solid-liquid, and washing and drying the precipitate to obtain the coupled thallium removal agent.

[0069] The coupled thallium removal agent prepared by the present invention is added to industrial wastewater containing thallium. Since thallium has natural geochemical sulfur- and iron-loving properties, free thallium in the wastewater will react to generate thallium sulfide and iron thallium sulfide forms after contacting with ferrous polysulfide FeSx in the coupled thallium removal agent, and the thallium is combined with the zeolite matrix through the original Fe-O bond and SO bond, so that the thallium in the industrial wastewater is captured and enters the amorphous ferrous polysulfide active material adsorbed on the surface of the zeolite to form a stable compound and be separated from the wastewater, thereby achieving the purpose of deep thallium removal from industrial thallium-containing wastewater.

[0070] The coupled thallium removal agent prepared by the present invention is added to industrial thallium-containing wastewater, and after encountering thallium ions with stronger sulfur affinity, dissociation and disproportionation reactions occur to generate insoluble substances of thallium sulfide and thallium iron sulfide, the structural formula of which is as follows:

[0071]

[0072] The invention provides a method for preparing a coupled thallium removal agent. The coupled thallium removal agent can be prepared by a two-step reaction, and the coupled thallium removal agent can be used to efficiently and deeply remove thallium from industrial thallium-containing wastewater by utilizing the dual coupling effects of physical adsorption and chemical reaction of the coupled thallium removal agent. The method has the advantages of simple preparation process and selective deep thallium removal.

[0073] The following is a detailed description of the preparation method of the coupled thallium removal agent provided by the present invention through examples.

[0074] The thallium-containing wastewater comes from a smelting enterprise, and the solution contains 128.39 μg / L thallium and pH = 5.5.

[0075] Example 1

[0076] The specific surface area of ​​the zeolite powder used as the synthetic raw material is 116 m 2 / g, the average particle size is 185 microns, and the malic acid and ferric sulfate are chemically pure.

[0077] The specific steps of the method for preparing the coupled thallium removal agent provided in this embodiment are as follows:

[0078] S1 slurry preparation: add 1000g zeolite powder and 40g malic acid into a beaker, pour in 3L water, stir evenly to obtain a malic acid precursor solution.

[0079] S2 price reduction: Add 20g of iron sulfate crystals to the precursor solution, maintain the reaction temperature at 40°C in a constant temperature water bath, and react for 1h under stirring.

[0080] S3 sulfidation evaporation: add Na2S / Na2S2 mixed crystals to the slurry obtained in step S2, wherein Na2S is 10g and Na2S2 is 10g, that is, the mass percentage of Na2S in the Na2S / Na2S2 mixed crystals is maintained at 50%. Heat to 80°C for sulfidation evaporation synthesis, and end evaporation when the volume of the residual solution is 400mL, and obtain a coupled thallium removal agent after solid-liquid separation.

[0081] The obtained coupled thallium removal agent was subjected to XRD, XPS and SEM analysis, and the obtained XRD graph, XPS graph and SEM graph were as follows: Figure 2 , Figure 3 ,and Figure 4 shown.

[0082] from Figure 2 It can be seen that the coupling thallium removal agent prepared in the embodiment of the present invention is mainly composed of silicon dioxide, with a large amount of FeS x , FeS2 phase. This confirms the synthetic goal of the material, that is, zeolite is used as the matrix, and its main component is silicon dioxide; at the same time, iron polysulfide compounds are obtained, including two main forms, and the intensity of the diffraction peak is weak, only a few hundred, which is much lower than the thousands of ordinary crystalline materials, indicating that the material is not highly crystalline and mostly exists in an amorphous form, which is exactly the form required in the present invention, and has high reactivity.

[0083] from Figure 3 It can be seen that the Fe in the coupled thallium removal agent prepared in the embodiment of the present invention mainly exists in the form of Fe-S bonds. This detection is a further confirmation and supplement to the XRD detection results, because the photon spectrum analysis only detects the morphology within a few tens of nanometers on the surface of the material, indicating that there are a large number of Fe and S bonds on the surface of the material, but no Si and O bonds, indicating that the effect of sulfidation evaporation is good, and a coupled adsorption material loaded with iron polysulfide is obtained.

[0084] from Figure 4It can be seen that the coupled thallium removal agent prepared in the embodiment of the present invention has a uniform morphology and is a porous aggregate particle. That is, the zeolite basically maintains its original good properties during the reaction process. It is a porous loose material with a large specific surface area. After being loaded, the surface properties remain unchanged, and the coupled thallium removal material is still a porous material.

[0085] 2 g of the coupled thallium removal agent prepared in this example was added to 1 L of thallium-containing wastewater, stirred and reacted at room temperature for 1 h, and then the residue and liquid were separated. The filtrate was sampled and analyzed, and the thallium content in the filtrate was 5.02 μg / L, and the calculated thallium removal rate was 96.09%.

[0086] Example 2

[0087] The specific surface area of ​​the zeolite powder used as the synthetic raw material is 116 m 2 / g, the average particle size is 185 microns, and the malic acid and ferric sulfate are chemically pure.

[0088] The specific steps of the method for preparing the coupled thallium removal agent provided in this embodiment are as follows:

[0089] S1 slurry preparation: add 1000g zeolite powder and 70g malic acid into a beaker, pour in 4L water, stir evenly to obtain a malic acid precursor solution.

[0090] S2 price reduction: Add 12g of iron sulfate crystals to the precursor solution, maintain the reaction temperature at 60°C in a constant temperature water bath, and react for 2h under stirring.

[0091] S3 sulfidation evaporation: Add Na2S / Na2S2 mixed crystals to the slurry obtained in step S2, wherein Na2S 5g, Na2S2 10g, i.e., keep the mass percentage of Na2S in the Na2S / Na2S2 mixed crystals at 33%. Heat to 100°C for sulfidation evaporation synthesis, and end evaporation when the volume of the residual solution is 400mL, and obtain a coupled thallium removal agent after solid-liquid separation.

[0092] 2 g of the coupled thallium removal agent prepared in this example was added to 1 L of thallium-containing wastewater, stirred and reacted at room temperature for 1 h, and then the residue and liquid were separated. The filtrate was sampled and analyzed, and the thallium content in the filtrate was 3.29 μg / L, and the calculated thallium removal rate was 97.44%.

[0093] Example 3

[0094] The specific surface area of ​​the zeolite used as the synthetic raw material is 116m 2 / g, the average particle size is 185 microns, and the malic acid and ferric sulfate are chemically pure.

[0095] The specific steps of the method for preparing the coupled thallium removal agent provided in this embodiment are as follows:

[0096] S1 slurry preparation: add 1000g zeolite powder and 100g malic acid into a beaker, pour in 6L water, stir evenly to obtain a malic acid precursor solution.

[0097] S2 price reduction: Add 60g of iron sulfate crystals to the precursor solution, maintain the reaction temperature at 80℃ in a constant temperature water bath, and react for 1h under stirring.

[0098] S3 sulfidation evaporation: add Na2S / Na2S2 mixed crystals to the slurry obtained in step S2, wherein Na2S 10g, Na2S 30g, i.e., keep the mass percentage of Na2S in the Na2S / Na2S2 mixed crystals at 25%. Heat to 90°C for sulfidation evaporation synthesis, and end evaporation when the volume of the residual solution is 800mL, and obtain the coupled thallium removal agent after solid-liquid separation.

[0099] 2 g of the coupled thallium removal agent prepared in this example was added to 1 L of thallium-containing wastewater, stirred and reacted at room temperature for 1 h, and then the residue and liquid were separated. The filtrate was sampled and analyzed, and the thallium content in the filtrate was 4.33 μg / L, and the calculated thallium removal rate was 96.63%.

[0100] Example 4

[0101] The specific surface area of ​​the zeolite used as the synthetic raw material is 372m 2 / g, the average particle size is 36 microns, and the malic acid and ferric sulfate are chemically pure.

[0102] The specific steps of the method for preparing the coupled thallium removal agent provided in this embodiment are as follows:

[0103] S1 slurry preparation: add 1000g zeolite powder and 70g malic acid into a beaker, pour in 2.5L water, stir evenly to obtain a malic acid precursor solution.

[0104] S2 price reduction: Add 20g of iron sulfate crystals to the precursor solution, maintain the reaction temperature at 70°C in a constant temperature water bath, and react for 1h under stirring.

[0105] S3 sulfidation evaporation: add Na2S / Na2S2 mixed crystals to the slurry obtained in step S2, wherein Na2S2g, Na2S210g, i.e., keep the mass percentage of Na2S in the Na2S / Na2S2 mixed crystals at 17%. Heat to 90°C for sulfidation evaporation synthesis, and end evaporation when the volume of the residual solution is 700mL, and obtain the coupled thallium removal agent after solid-liquid separation.

[0106] 2 g of the coupled thallium removal agent prepared in this example was added to 1 L of thallium-containing wastewater, stirred and reacted at room temperature for 1 h, and then the residue and liquid were separated. The filtrate was sampled and analyzed, and the thallium content in the filtrate was 4.27 μg / L, and the calculated thallium removal rate was 96.67%.

[0107] Example 5

[0108] The specific surface area of ​​the zeolite used as the synthetic raw material is 214m 2 / g, the average particle size is 76 microns, and the malic acid and ferric sulfate are chemically pure.

[0109] The specific steps of the method for preparing the coupled thallium removal agent provided in this embodiment are as follows:

[0110] S1 slurry preparation: add 1000g zeolite powder and 50g malic acid into a beaker, pour in 5L water, stir evenly to obtain a malic acid precursor solution.

[0111] S2 price reduction: Add 30g of iron sulfate crystals to the precursor solution, maintain the reaction temperature at 50°C in a constant temperature water bath, and react for 2h under stirring.

[0112] S3 sulfidation evaporation: Add Na2S / Na2S2 mixed crystals to the slurry obtained in step S2, wherein Na2S is 5g and Na2S2 is 16g, i.e., the mass percentage of Na2S in the Na2S / Na2S2 mixed crystals is maintained at 24%. Heat to 100°C for sulfidation evaporation synthesis, and terminate evaporation when the volume of the residual solution is 2.5L. After solid-liquid separation, a coupled thallium removal agent is obtained.

[0113] 2 g of the coupled thallium removal agent prepared in this example was added to 1 L of thallium-containing wastewater, stirred and reacted at room temperature for 1 h, and then the residue and liquid were separated. The filtrate was sampled and analyzed, and the thallium content in the filtrate was 2.10 μg / L, and the calculated thallium removal rate was 98.36%.

[0114] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A coupled thallium removal agent, characterized in that: It includes zeolite powder as a carrier and amorphous ferrous polysulfide active material combined on the surface of the zeolite powder; Wherein, the amorphous ferrous polysulfide active material is bonded to the zeolite via an iron-oxygen bond and a sulfur-oxygen bond; The structural formula of the coupled thallium removal agent includes:

2. The coupling thallium removal agent according to claim 1, characterized in that: The specific surface area of ​​the zeolite powder is 80 to 400 m 2 / g, and the average particle size is 10 to 300 microns.

3. A method for preparing the coupling thallium removal agent according to claim 1 or 2, characterized in that: The following steps are involved: adding malic acid solution to zeolite powder to form a weakly acidic precursor solution; Adding ferric sulfate crystals to the precursor solution, stirring and reacting to obtain a ferrous malate complex solution; Adding Na2S / Na2S2 mixed crystals to the mixed solution, heating to dissolve and evaporate and crystallize, to obtain a residual solution containing amorphous ferrous polysulfide active material adsorbed on the surface of zeolite powder; The residual liquid is separated into solid and liquid to obtain a coupled thallium removal agent.

4. The method for preparing the coupling thallium removal agent according to claim 3, characterized in that: The malic acid in the malic acid solution accounts for 3% to 10% of the mass of the zeolite powder, and the water in the malic acid solution accounts for 2.5 to 6 times of the mass of the zeolite powder.

5. The method for preparing the coupling thallium removal agent according to claim 3, characterized in that: The iron sulfate crystals account for 1% to 6% of the mass of the zeolite powder.

6. The method for preparing the coupling thallium removal agent according to claim 3, characterized in that: The reaction temperature after adding ferric sulfate crystals into the precursor solution is 40-80° C., and the reaction time is 0.5-2 hours.

7. The method for preparing the coupling thallium removal agent according to claim 3, characterized in that: The added amount of the Na2S / Na2S2 mixed crystals is 0.6 to 1.3 times the mass of ferric sulfate.

8. The method for preparing the coupling thallium removal agent according to claim 7, characterized in that: The mass percentage of Na2S in the Na2S / Na2S2 mixed crystal is 10-50%.

9. The method for preparing the coupling thallium removal agent according to claim 3, characterized in that: The temperature during the heating and evaporation process is 80-100°C.

10. The method for preparing the coupling thallium removal agent according to claim 9, characterized in that: The evaporation rate of the evaporated solution is 50-90%.

Citation Information

Cited By

  • Composite material for adsorbing heavy metal thallium and preparation method thereof

    CN121623736A