Anti-seepage low-shrinkage mortar and preparation method thereof
By combining low-thermal silicate cement, micro-expanded silicate cement and gypsum hydration products, a dense structure is formed, and a hydrophobic layer is formed using glyceryl stearate and sodium methyl silicate, the traditional waterproof mortar is solved by solving the low strength and shrinkage of traditional waterproof mortar. The major problem is that low shrinkage and high anti-seepage mortar can be achieved, avoiding building leakage.
Patent Information
- Application Number
- CN202411208160.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-30
AI Technical Summary
Traditional inorganic waterproof mortars have problems such as low strength, large shrinkage and insufficient structural density, resulting in frequent building leakage.
Low-thermal silicate cement, micro-expanded silicate cement and gypsum hydration products are combined to form a dense structure, and a hydrophobic film is formed through saponification reaction of glycerol stearate, and a hydrophobic layer is formed by combining sodium methyl silicate to enhance the material Anti-seepage performance.
The mortar with low shrinkage and high anti-seepage performance is achieved, which avoids material cracking and leakage problems, and improves the waterproof performance and durability of the building.
Smart Images

Figure QLYQS_1 
Figure BDA0005019615950000011 
Figure BDA0005019615950000021
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of inorganic non-metallic materials, and in particular to an anti-seepage low-shrinkage mortar and a preparation method thereof. Background Art
[0002] Building leakage has always been a difficult problem, often occurring in places where water easily accumulates, such as bathrooms, balconies, exterior walls, and basements. According to incomplete statistics: 35% of buildings leak within two years after completion of construction, and 55% of houses cannot be used normally due to leakage. Common waterproof materials on the market are divided into inorganic waterproof materials and organic waterproof materials. The advantages of inorganic waterproof mortar are low cost, no toxic or harmful substances in the materials, and simple construction. Waterproof mortar also has certain defects, such as low strength, large shrinkage, and insufficient structural density. Traditional inorganic waterproof mortar uses ordinary Portland cement as the main cementing material, but ordinary Portland cement has a large shrinkage rate and is easy to crack, resulting in it no longer having a waterproof effect; the shrinkage rate of low-heat Portland cement at each age is 50% to 70% of that of ordinary Portland cement, and the shrinkage rate after 28 days basically does not change. The hydration of low-heat Portland cement is slow, and its hydration product is denser and more durable; therefore, the present invention uses low-heat Portland cement as the main cementing material to prepare anti-seepage and low-shrinkage mortar. Summary of the invention
[0003] In order to overcome the defects and shortcomings of the existing technologies, the present invention provides an anti-seepage low-shrinkage mortar and a preparation method thereof. The anti-seepage low-shrinkage mortar selects green inorganic materials, combines the characteristics of slow hydration of low-heat silicate cement, micro-expansion of high-magnesium low-heat silicate cement, and micro-expansion of calcium sulfonate products formed between gypsum and cement hydration products, and the micro-expansion characteristics alleviate the shrinkage problem of the material and enable the material to form a dense structure; and through the saponification reaction of the hydrophobic material glyceryl stearate under alkaline conditions, a hydrophobic film is formed on the surface of the cementitious material, and sodium methyl silicate forms a hydrophobic layer on the surface of the fine aggregate, so that the material has excellent hydrophobic and anti-seepage properties.
[0004] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0005] The present invention discloses an anti-seepage low-shrinkage mortar, comprising the following raw materials in parts by mass:
[0006]
[0007]
[0008] In some implementations of the present invention, the anti-seepage low-shrinkage cementitious material includes the following components by mass: 15-30 parts of low-heat silicate cement, 15-35 parts of high-magnesium low-heat silicate cement, 5-20 parts of fast-hardening sulphoaluminate cement, 6-18 parts of silica fume, 8-12 parts of fly ash, 3-8 parts of blast furnace slag powder, 3-10 parts of gypsum, 2-8 parts of talc, 1-5 parts of glyceryl stearate, 0.3-0.8 parts of sodium silicate, 0.5-2.5 parts of defoamer, 1-5 parts of water reducer, 0.3-0.8 parts of lithium carbonate, 0.8-2 parts of hydroxypropyl methylcellulose, and 1-5 parts of redispersible latex powder;
[0009] Preferably, the anti-seepage low-shrinkage cementitious material includes the following components in parts by mass: 20 parts of low-heat silicate cement, 20 parts of high-magnesium low-heat silicate cement, 10 parts of fast-hardening sulphoaluminate cement, 10 parts of silica fume, 10 parts of fly ash, 5 parts of blast furnace slag powder, 5 parts of gypsum, 5 parts of talc, 2 parts of glyceryl stearate, 0.5 parts of sodium silicate, 1 part of defoamer, 2 parts of water reducer, 0.5 parts of lithium carbonate, 1 part of hydroxypropyl methylcellulose, and 2 parts of redispersible latex powder.
[0010] In some implementations of the present invention, the mineral composition of the low heat silicate cement is: 20-35wt% C 3 S, 40-60wt% C 2 S, 2-7 wt% C 3 A. 10-20wt% C 4 AF; The mineral composition of the high magnesium low heat silicate cement is: 20 to 35wt% C 3 S, 35-60wt% C 2 S, 1-8 wt% C 3 A. 10~25wt%C 4 AF, MgO content is 3-8wt%; the mineral composition of the rapid hardening sulphoaluminate cement is: 50-70wt% C 4 A 3 S, 10-35wt%C 2 S, 3-8 wt% C 4 AF.
[0011] In some embodiments of the present invention, the blast furnace slag powder is S95 grade blast furnace slag powder with a specific surface area of 500 to 700 m 2 / kg.
[0012] In some embodiments of the present invention, the gypsum is industrial solid waste phosphogypsum with a specific surface area of 500 to 700 m 2 / kg.
[0013] In some embodiments of the present invention, the silicon content of the silica fume is more than 90%, and the specific surface area is 15 to 19 m 2 / g.
[0014] In some implementations of the present invention, the talcum powder is industrial grade talcum powder with a fineness of 3000 mesh.
[0015] In some implementations of the present invention, the fly ash is Class I fly ash.
[0016] In some implementations of the present invention, the machine-made sand grading is: 2.36 mm standard sieve residue 16%, 1.18 mm standard sieve residue 14%, 0.6 mm standard sieve residue 29%, 0.3 mm standard sieve residue 23%, 0.075 mm standard sieve residue 18%, and the porosity is 36%.
[0017] In some implementations of the present invention, the water repellent is sodium methyl silicate with a solid content of 40 wt%.
[0018] The present invention also discloses a method for preparing an anti-seepage low-shrinkage mortar, comprising the following steps:
[0019] S1. Low-heat silicate cement, high-magnesium low-heat silicate cement, rapid-hardening sulphoaluminate cement, silica fume, fly ash, blast furnace slag powder, gypsum, talcum powder and stearin are uniformly mixed and ball-milled to obtain a powder; preferably, the ball-milling speed is 200-400 r / s, the ball-milling time is 10-40 min, and the powder particle size is 5-20 μm;
[0020] S2. Divide the water into two parts by weight, add the water repellent to one part of the water to obtain a water repellent dilution solution, and keep the other part of the water for standby use;
[0021] S3, stirring the sand at a low speed, spraying the water-repellent dilution during the stirring process to obtain fine aggregate; preferably, the low-speed stirring time is 120 seconds;
[0022] S4, pour the powder and admixture obtained in S1 into the fine aggregate obtained in S3 and stir at a low speed for 60 seconds, then add another portion of water in S2 and continue stirring at a low speed for 30 seconds, and finally stir rapidly for 60 seconds to obtain a mixed slurry;
[0023] S5, pouring the mixed slurry into a mold, vibrating and shaping it, curing, and demoulding, so as to obtain the anti-seepage low shrinkage mortar.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1. The present invention mainly adopts low-heat silicate cement and high-magnesium low-heat silicate cement. Low-heat silicate cement has the characteristics of small shrinkage and low hydration heat, and low hydration heat can alleviate material cracking; high-magnesium low-heat silicate cement has a micro-expansion effect, and the calcium sulfonate hydration product generated by adding gypsum also has a micro-expansion effect, which effectively avoids the problem of large material shrinkage.
[0026] 2. The present invention selects glyceryl stearate as a hydrophobic agent, and grinds the cementitious material and glyceryl stearate together so that the surface of the cementitious material particles is evenly coated with glyceryl stearate. Under alkaline conditions, glyceryl stearate is hydrated into stearate and glycerol to form a hydrophobic film, thereby improving the anti-seepage performance of the cementitious material. The fine aggregate is reorganized by screening, and the best gradation is obtained by adopting a close stacking model. Sodium methyl silicate is evenly sprayed on the surface of the fine aggregate to form a hydrophobic layer on the surface, so that the fine aggregate has anti-seepage performance. Talc has a certain hydrophobicity, and ultrafine silica fume and talc can fill the capillary pores inside the fine aggregate structure, reduce the porosity, form a denser structure inside, and further improve the anti-seepage performance.
[0027] 3. The present invention ensures the waterproof effect of fine aggregate while ensuring the anti-seepage effect of powder, and the mortar has excellent waterproof performance. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0029] In an embodiment of the present invention, the anti-seepage low-shrinkage cementitious material includes the following components in parts by mass: 20 parts of low-heat silicate cement, 20 parts of high-magnesium low-heat silicate cement, 10 parts of fast-hardening sulphoaluminate cement, 10 parts of silica fume, 10 parts of fly ash, 5 parts of blast furnace slag powder, 5 parts of gypsum, 5 parts of talc, 2 parts of glyceryl stearate, 0.5 parts of sodium silicate, 1 part of defoamer, 2 parts of water reducer, 0.5 parts of lithium carbonate, 1 part of hydroxypropyl methylcellulose, and 2 parts of redispersible latex powder.
[0030] In the embodiment of the present invention, the mineral composition of hot silicate cement is: 20-35wt% C 3 S, 40-60wt% C 2 S, 2-7 wt% C 3 A. 10-20wt% C 4 AF; The mineral composition of high magnesium low heat silicate cement is: 20-35wt% C 3 S, 35-60wt% C 2 S, 1-8 wt% C 3 A. 10~25wt%C 4 AF, MgO content is 3-8wt%; the mineral composition of rapid hardening sulphoaluminate cement is: 50-70wt% C 4 A 3 S, 10-35wt%C 2S, 3-8 wt% C 4 AF.
[0031] In the embodiment of the present invention, the blast furnace slag powder is S95 grade blast furnace slag powder with a specific surface area of 500-700m 2 / kg.
[0032] In the embodiment of the present invention, the gypsum is industrial solid waste phosphogypsum with a specific surface area of 500-700m 2 / kg.
[0033] In the embodiment of the present invention, the silicon content of the silica fume is more than 90%, and the specific surface area is 15 to 19 m 2 / g.
[0034] In the embodiment of the present invention, the talcum powder is industrial grade talcum powder with a fineness of 3000 mesh.
[0035] In the embodiment of the present invention, the fly ash is Class I fly ash.
[0036] In the embodiment of the present invention, the machine-made sand grading is: 2.36 mm standard sieve residue 16%, 1.18 mm standard sieve residue 14%, 0.6 mm standard sieve residue 29%, 0.3 mm standard sieve residue 23%, 0.075 mm standard sieve residue 18%, and the porosity is 36%.
[0037] In the embodiment of the present invention, the water repellent is sodium methyl silicate, and the solid content is 40wt%.
[0038] In an embodiment of the present invention, a method for preparing an anti-seepage low shrinkage mortar comprises the following steps:
[0039] S1. Low-heat silicate cement, high-magnesium low-heat silicate cement, rapid-hardening sulphoaluminate cement, silica fume, fly ash, blast furnace slag powder, gypsum, talcum powder and stearic acid glycerol are uniformly mixed and ball-milled in a ball mill at a ball-milling speed of 200 to 400 r / s for a ball-milling time of 10 to 40 min to obtain a powder having a particle size of 5 to 20 μm;
[0040] S2. Divide the water into two parts by weight, add the water repellent to one part of the water to obtain a water repellent dilution solution, and keep the other part of the water for standby use;
[0041] S3, stirring the sand at a low speed, spraying the water-repellent dilution during the stirring process to obtain fine aggregate; preferably, the low-speed stirring time is 120 seconds;
[0042] S4, pour the powder and admixture obtained in S1 into the fine aggregate obtained in S3 and stir at a low speed for 60 seconds, then add another portion of water in S2 and continue stirring at a low speed for 30 seconds, and finally stir rapidly for 60 seconds to obtain a mixed slurry;
[0043] S5, pouring the mixed slurry into a mold, vibrating and shaping it, curing, and demoulding, so as to obtain the anti-seepage low shrinkage mortar.
[0044] Example 1
[0045] As a preferred embodiment of the present invention, the anti-seepage low-shrinkage mortar disclosed in this embodiment has a raw material composition as shown in Table 1.
[0046] Table 1 Raw material composition of Example 1 anti-seepage low shrinkage mortar
[0047] Raw material name Mass parts / parts Anti-seepage low shrinkage cementitious material 50 Machine-made sand 180 Water repellent 3 water 60
[0048] According to the mass fractions of each raw material in Table 1, the anti-seepage low-shrinkage mortar #1 was obtained by adopting the preparation method.
[0049] Example 2
[0050] As a preferred embodiment of the present invention, the anti-seepage low-shrinkage mortar disclosed in this embodiment has a raw material composition as shown in Table 2.
[0051] Table 2 Raw material composition of Example 2 anti-seepage low shrinkage mortar
[0052]
[0053]
[0054] According to the mass fractions of each raw material in Table 2, the anti-seepage low-shrinkage mortar #2 was obtained by adopting the preparation method.
[0055] Example 3
[0056] As a preferred embodiment of the present invention, the anti-seepage low-shrinkage mortar disclosed in this embodiment has a raw material composition as shown in Table 3.
[0057] Table 3 Raw material composition of the anti-seepage low shrinkage mortar of Example 3
[0058] Raw material name Mass parts / parts Anti-seepage low shrinkage cementitious material 45 Machine-made sand 145 Water repellent 2 water 40
[0059] According to the mass fractions of each raw material in Table 3, the preparation method was adopted to obtain anti-seepage low-shrinkage mortar #3.
[0060] Example 4
[0061] As a preferred embodiment of the present invention, the anti-seepage low-shrinkage mortar disclosed in this embodiment has a raw material composition as shown in Table 4.
[0062] Table 4 Raw material composition of Example 4 anti-seepage low shrinkage mortar
[0063] Raw material name Mass parts / parts Anti-seepage low shrinkage cementitious material 53 Machine-made sand 175 Water repellent 2.5 water 55
[0064] According to the mass fractions of each raw material in Table 4, the preparation method was adopted to obtain anti-seepage low-shrinkage mortar #4.
[0065] Comparative Example 1
[0066] In this comparative example, except that ordinary Portland cement is used to replace low-heat Portland cement and high-magnesium low-heat Portland cement, the rest is the same as Example 1 to obtain comparative mortar #1.
[0067] Comparative Example 2
[0068] In this comparative example, except that ordinary silicate hydrophobic agent was used to replace fatty acid glyceryl ester as the hydrophobic agent, the rest was the same as Example 1, and comparative mortar #2 was obtained.
[0069] Comparative Example 3
[0070] In this comparative example, except that polysiloxane was used to replace sodium methyl silicate as the water repellent, the rest was the same as Example 1, and a comparative mortar #3 was obtained.
[0071] Test Case
[0072] The mortars of Examples 1 to 4 and Comparative Examples 1 to 3 were subjected to anti-permeability tests and shrinkage tests, respectively.
[0073] Permeability test: The permeability test of mortar is carried out according to JGJ / T70-2009 "Standard for Test Methods of Basic Performance of Building Mortar". The permeability test of mortar is tested by SJS-1.5S digital display permeability tester; the upper diameter of the specimen is 70mm, the lower diameter is 80mm, and the height is 30mm. After molding, it is demoulded after standing at 20℃ for 24h, and then placed in a curing pool at 20℃ for 14d. After the specimen reaches the curing age, it is taken out and the surface is dried. After being sealed with wax, it is loaded into the permeameter for permeability test. During the test, the pressure is increased from 0.2MPa, kept constant for 2h, and then increased to 0.3MPa. After that, it is increased by 0.1MPa every 1h. The test is stopped when water seepage occurs on the surface of one of the three specimens.
[0074] Shrinkage rate and tensile bond strength test: refer to JGJ70-90 "Test methods for basic properties of building mortar".
[0075] Flexural strength and compressive strength test: refer to GBT17671-2021 "Test method for strength of cement mortar". Molded with a 40*40*160mm triple mold, cured in a curing box with a temperature of 20℃±1℃ and a humidity of not less than 90%.
[0076] The relevant test results are shown in Table 5.
[0077] Table 5 Test results of mortars of Examples 1 to 4 and Comparative Examples 1 to 3
[0078]
[0079]
[0080] According to Table 5, the mortar obtained according to the formula provided by the present invention has excellent anti-seepage performance, low shrinkage rate, and the shrinkage of the mortar does not change substantially after 28 days; the compression ratio is less than 3.0, which further illustrates that the material has good flexibility, is conducive to improving crack resistance, and effectively avoids the problem of material cracking.
[0081] Finally, it should be noted that the above embodiments are only preferred embodiments of the present invention to illustrate the technical solutions of the present invention, rather than limiting them, and certainly not limiting the patent scope of the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. In other words, any changes or modifications made to the main design concept and spirit of the present invention that have no substantive significance, and the technical problems they solve are still consistent with the present invention, should be included in the protection scope of the present invention. In addition, the direct or indirect application of the technical solutions of the present invention in other related technical fields is also included in the patent protection scope of the present invention.
Claims
1. An anti-seepage low shrinkage mortar, characterized in that: Including the following raw materials by mass:
2. The anti-seepage low shrinkage mortar according to claim 1, characterized in that: The anti-seepage low-shrinkage cementitious material includes the following components in parts by mass: 15-30 parts of low-heat silicate cement, 15-35 parts of high-magnesium low-heat silicate cement, 5-20 parts of fast-hardening sulphoaluminate cement, 6-18 parts of silica fume, 8-12 parts of fly ash, 3-8 parts of blast furnace slag powder, 3-10 parts of gypsum, 2-8 parts of talc, 1-5 parts of glyceryl stearate, 0.3-0.8 parts of sodium silicate, 0.5-2.5 parts of defoaming agent, 1-5 parts of water reducing agent, 0.3-0.8 parts of lithium carbonate, 0.8-2 parts of hydroxypropyl methylcellulose and 1-5 parts of redispersible latex powder.
3. The anti-seepage low shrinkage mortar according to claim 2, characterized in that: The anti-seepage low-shrinkage cementitious material includes the following components in parts by mass: 20 parts of low-heat silicate cement, 20 parts of high-magnesium low-heat silicate cement, 10 parts of fast-hardening sulphoaluminate cement, 10 parts of silica fume, 10 parts of fly ash, 5 parts of blast furnace slag powder, 5 parts of gypsum, 5 parts of talc, 2 parts of glyceryl stearate, 0.5 parts of sodium silicate, 1 part of defoamer, 2 parts of water reducer, 0.5 parts of lithium carbonate, 1 part of hydroxypropyl methylcellulose, and 2 parts of redispersible latex powder.
4. The anti-seepage low shrinkage mortar according to claim 2, characterized in that: The mineral composition of the low-heat silicate cement is: 20-35wt% C3S, 40-60wt% C2S, 2-7wt% C3A, 10-20wt% C4AF; the mineral composition of the high-magnesium low-heat silicate cement is: 20-35wt% C3S, 35-60wt% C2S, 1-8wt% C3A, 10-25wt% C4AF, and the MgO content is 3-8wt%; the mineral composition of the fast-hardening sulphoaluminate cement is: 50-70wt% C4A3S, 10-35wt% C2S, 3-8wt% C4AF.
5. The anti-seepage low shrinkage mortar according to claim 2, characterized in that: The blast furnace slag powder is S95 grade blast furnace slag powder with a specific surface area of 500-700m 2 / kg; the gypsum is industrial solid waste phosphogypsum with a specific surface area of 500-700m 2 / kg.
6. The anti-seepage low shrinkage mortar according to claim 2, characterized in that: The silicon content of the silica fume is more than 90%, and the specific surface area is 15 to 19 m 2 / g.
7. The anti-seepage low shrinkage mortar according to claim 2, characterized in that: The talcum powder is industrial-grade talcum powder with a fineness of 3000 mesh; the fly ash is grade I fly ash.
8. The anti-seepage low-shrinkage mortar according to claim 1, characterized in that: The machine-made sand grading is: 2.36mm standard sieve residue 16%, 1.18mm standard sieve residue 14%, 0.6mm standard sieve residue 29%, 0.3mm standard sieve residue 23%, 0.075mm standard sieve residue 18%, and the porosity is 36%.
9. The anti-seepage low shrinkage mortar according to claim 1, characterized in that: The water repellent is sodium methyl silicate, and the solid content is 40wt%.
10. A method for preparing an anti-seepage low-shrinkage mortar according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. Low-heat silicate cement, high-magnesium low-heat silicate cement, rapid-hardening sulphoaluminate cement, silica fume, fly ash, blast furnace slag powder, gypsum, talcum powder and stearin are uniformly mixed and ball-milled to obtain a powder; preferably, the ball-milling speed is 200-400 r / s, the ball-milling time is 10-40 min, and the powder particle size is 5-20 μm; S2. Divide the water into two parts by weight, add the water repellent to one part of the water to obtain a water repellent dilution solution, and keep the other part of the water for standby use; S3, stirring the sand at a low speed, spraying the water-repellent dilution during the stirring process to obtain fine aggregate; preferably, the low-speed stirring time is 120 seconds; S4, pour the powder and admixture obtained in S1 into the fine aggregate obtained in S3 and stir at a low speed for 60 seconds, then add another portion of water in S2 and continue stirring at a low speed for 30 seconds, and finally stir rapidly for 60 seconds to obtain a mixed slurry; S5, pouring the mixed slurry into a mold, vibrating and shaping it, curing, and demoulding, so as to obtain the anti-seepage low shrinkage mortar.
Citation Information
Patent Citations
High-magnesium low-heat portland cement clinker aggregate and preparation method thereof
CN101041560A
Machine-spraying light-weight plastering mortar and preparation method thereof
CN107619239A
Impervious cement construction mortar and production method thereof
CN107902993A
Method for preparing impervious hydrophobic cement from oleic acid-modified fly ash
CN108249850A
Sprayable, waterproof, anticorrosive and erosion-resistant high-strength mortar and using method thereof
CN110668774A