Polyacrylonitrile-based modified material as well as preparation method and application thereof

By swelling polyacrylonitrile in graft monomer solution and irradiating it to initiate graft polymerization, the problem of low utilization rate of graft monomer in heterogeneous graft polymerization is solved, and efficient polymer material modification is achieved and the application of adsorption separation of photothermal conversion materials.

CN118930750APending Publication Date: 2024-11-12SHANGHAI UNIV +1

Patent Information

Application Number
CN202411039775.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the process of modification of existing polymer materials, heterogeneous graft polymerization leads to low utilization rate of graft monomers and slow grafting rate, and limited applications in the fields of adsorption and separation photothermal conversion.

Method used

Polyacrylonitrile is used to swell in a solution containing graft monomer, and then graft polymerization is initiated by irradiation to increase the contact rate between graft monomer and polymer substrate, and achieve efficient modification.

Benefits of technology

It improves polymer modification efficiency, high material functional group density, high graft monomer utilization rate, reduces material preparation cost, and reduces waste liquid generation, making it suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930750A_ABST
    Figure CN118930750A_ABST
Patent Text Reader

Abstract

The invention relates to a polyacrylonitrile-based modified material as well as a preparation method and application thereof. The preparation method comprises the following steps: S1, soaking polyacrylonitrile in a solution containing a grafting monomer for swelling; s2, the polyacrylonitrile obtained after swelling in the step S1 is subjected to a graft polymerization reaction initiated by irradiation, and the polyacrylonitrile-based modified material is obtained. Compared with the prior art, the preparation method disclosed by the invention has the advantages that by utilizing a polymer swelling and graft polymerization technology, more grafting monomers enter the polymer in a polymer swelling state and are in full contact with the polymer, so that a grafting reaction interface is maximized, and the polymer modification efficiency and the monomer utilization rate are improved; and the prepared modified material is high in functional group density and good in performance, and is a new idea for heterogeneous graft polymerization modification of high polymer materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymer materials, and in particular to a modified material based on polyacrylonitrile and a preparation method and application thereof. Background Art

[0002] Heterogeneous grafting polymerization is usually used to modify polymer materials such as fibers, films, and non-woven fabrics. However, in this reaction system, the grafting monomer and the modified substrate exist in the liquid and solid phases respectively. Since the diffusion of the monomer from the interface between the two phases to the interior of the substrate is hindered, the utilization rate of the grafting monomer is low and the grafting rate is slow during the heterogeneous grafting polymerization process.

[0003] At present, there is a new idea of ​​swelling the polymer and then carrying out a grafting polymerization reaction in the swollen state. For example, the existing patent CN111749016A discloses a polyethylene polymerization grafting impregnation liquid and a method for ultra-high molecular weight polyethylene polymerization grafting modification. The grafting impregnation liquid includes a polyethylene grafting monomer, a polymerization initiator, a catalyst, a ligand and a photoinitiator. The grafting monomer is used to swell the ultra-high molecular weight polyethylene, and then the grafting reaction is directly carried out.

[0004] However, since the substrates used in adsorption separation, photothermal conversion, etc. are not easy to swell, the modification of polymers in a swollen state is still a blank in the fields of adsorption separation materials, photothermal conversion, etc. Summary of the invention

[0005] The purpose of the present invention is to provide a modified material based on polyacrylonitrile and its preparation method and application in order to overcome the problems of low utilization rate of heterogeneous graft polymerization monomers in the preparation process of existing polymer modified adsorption materials.

[0006] The purpose of the present invention can be achieved by the following technical solutions:

[0007] One of the technical solutions of the present invention is to provide a method for preparing a modified material based on polyacrylonitrile, comprising the following steps:

[0008] S1, soaking polyacrylonitrile in a solution containing a grafting monomer to swell;

[0009] S2. Irradiate the polyacrylonitrile that has been swollen in step S1 to initiate a graft polymerization reaction of the monomers, thereby obtaining a modified material based on polyacrylonitrile.

[0010] In some specific embodiments, in step S1, the molecular weight of the polyacrylonitrile is M w (8-300)×10 4 .

[0011] In some specific embodiments, in step S1, the morphology of the polyacrylonitrile is selected from any one of powder, resin particles, film, fiber and non-woven fabric.

[0012] In some specific embodiments, in step S1, the final concentration of the grafting monomer in the solution is 10 wt%-40 wt%.

[0013] In some specific embodiments, in step S1, the grafting monomer is selected from any one or more of acrylic acid, methacrylic acid, acrylonitrile, styrene, 4-chloromethylstyrene, glycidyl methacrylate, 4-hydroxybutyl acrylate glycidyl ether, hydroxyethyl acrylate, vinylaniline, vinylpyrrole, polyvinyl alcohol, and polyacrylamide.

[0014] In some specific embodiments, in step S1, the solution is selected from any one or more of methanol, ethanol, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, ethyl acetate, acetone, benzene, chloroform, and water.

[0015] In some specific embodiments, in step S1, the swelling time is 4-48 hours, the swelling temperature is 10-60° C., and the swelling method is stirring swelling or static swelling.

[0016] In some specific embodiments, in step S2, the irradiation source used for irradiation is an electron accelerator or cobalt-60, and the irradiation method is co-irradiation with liquid.

[0017] In some specific embodiments, in step S2, when the irradiation source is an electron accelerator, the irradiation dose rate is 1-5 kGy / s; when the irradiation source is cobalt-60, the irradiation dose rate is 1-5 kGy / h.

[0018] In some specific embodiments, in step S2, the irradiation absorbed dose is 5-300 kGy, the irradiation temperature is room temperature, and the irradiation atmosphere is air, nitrogen or vacuum atmosphere.

[0019] The second technical solution of the present invention is to provide a modified material based on polyacrylonitrile, which is obtained based on the preparation method described in one of the above technical solutions.

[0020] The third technical solution of the present invention is to provide an application of a modified material based on polyacrylonitrile as described in the second technical solution above, wherein the modified material based on polyacrylonitrile is used as an adsorption material and / or a photothermal conversion material.

[0021] In some specific embodiments, the adsorption material and the photothermal conversion material are obtained by post-processing the modified material based on polyacrylonitrile:

[0022] When the modified material based on polyacrylonitrile has an epoxy group, a ring-opening reaction is performed;

[0023] When the polyacrylonitrile-based modified material has a cyano group, an oximation reaction is performed;

[0024] When the modified material based on polyacrylonitrile has a chlorophenyl group, a sulfonation reaction and / or a quaternization reaction is performed;

[0025] Alternatively, aniline is added to the modified material based on polyacrylonitrile to perform a polyaniline modification reaction, or pyrrole is added to perform a polypyrrole modification reaction.

[0026] In some specific embodiments, the modified polyacrylonitrile-based material is used as an adsorbent material to adsorb metal ions in a metal ion-containing aqueous solution.

[0027] In some specific embodiments, the modified polyacrylonitrile-based material is used as a photothermal conversion material to desalinate seawater or concentrated brine.

[0028] The polyacrylonitrile (PAN) used in the present invention is a polymer with a strong polar group -CN formed by the polymerization of acrylonitrile monomers. The acrylonitrile units in the PAN molecular chain are mainly connected head to tail, and the carbon atoms connected to the -CN group are separated by a methylene group. Since the atomic arrangement tends to be in a state with lower energy, the PAN main chain presents a spiral spatial stereo conformation. The PAN structure is two-dimensionally ordered, and the ordered and disordered regions permeate each other. The aggregated structure is also divided into several types: amorphous, mesogens, crystalline, and entangled networks. The strong polar group -CN and the spiral spatial stereo conformation determine that PAN can be dissolved in some organic solvents. However, the swelling and solubility of the polymer are determined by their molecular weight, molecular weight distribution and the degree of branching of the macromolecule. At the same time, the aggregated structure of the polymer greatly affects its swelling and dissolution. PAN has a larger molecular weight and is difficult to dissolve, which provides sufficient space for its swelling. Currently, commercial high molecular weight PAN can be obtained through free radical chain polymerization. The PAN molecular weight M prepared by suspension polymerization, mixed solvent method, aqueous precipitation method, etc. w Up to 300×10 4 The ability to make PAN swell in specific solvents can provide a substrate for swelling graft polymerization and opportunities for new adsorption separation materials and photothermal conversion materials.

[0029] In the preparation method provided by the present invention, small molecules such as solvents and grafted monomers are continuously infiltrated during the swelling process of the polyacrylonitrile substrate, so that the volume of the swollen polyacrylonitrile material is continuously increased, and the movement of the macromolecular chain segments is enhanced. The polyacrylonitrile substrate is swollen with a mixed solution containing a specific grafted monomer, and a graft polymerization reaction is carried out in the swollen state, so that the grafted monomer is fully in contact with the polymer substrate, the grafted polymerization reaction cross section is maximized, the grafted monomer can be utilized to the greatest extent, and the grafted polymerization modification efficiency of the material is high.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] (1) The present invention utilizes polymer swelling and grafting polymerization technology to allow the grafted monomer to enter the interior of the polymer more when the polymer is swollen and fully contact the polymer, thereby maximizing the grafting reaction interface and improving the polymer modification efficiency. The prepared modified material has a high functional group density, which is a new idea for heterogeneous grafting polymerization modification of polymer materials.

[0032] (2) In the present invention, only the grafted monomer enters the interior of the polymer substrate, and the grafted monomer and solvent in the prepared solution that are not swollen into the interior of the substrate are not irradiated and can be recycled; and the solution containing the grafted monomer will not be homopolymerized and can be recycled. The entire irradiation graft polymerization process produces very little waste liquid, and is expected to be mass-produced and promoted for application.

[0033] (3) The swelling and grafting polymerization involved in the present invention is simple to operate, has a high utilization rate of grafting monomers, low monomer consumption during batch material synthesis, and low material preparation cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 These are SEM images of the polyacrylonitrile substrate fiber, swollen polyacrylonitrile fiber, grafted polymer fiber, and amine oxime modified fiber in Example 3. DETAILED DESCRIPTION

[0035] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0036] In the following examples and comparative examples, unless otherwise specified, raw materials or processing techniques are conventional commercially available raw materials or conventional processing techniques in the art.

[0037] Embodiment 1:

[0038] This embodiment provides a method for preparing a modified material based on polyacrylonitrile, comprising the following steps:

[0039] (1) Preparation of monomer solution: Prepare 10 mL of a mixed solution of N,N-dimethylformamide / water (1:1, v:v) containing acrylic acid. The concentration of acrylic acid is C m It is 30wt%.

[0040] (2) 1 g of polyacrylonitrile powder (molecular weight M w 8×10 4 ) was placed in the prepared monomer solution and stirred at 40°C for 8 hours to swell. After the swelling was completed, the polyacrylonitrile powder was filtered from the monomer solution and weighed, with a mass of 3.96 g. The monomer loading (m m ) is calculated by the following formula:

[0041] m m =(m s -m0)*C m , where m0,m s are the mass of the material before and after swelling (g), C m is the monomer concentration (wt %) in the grafting monomer solution.

[0042] In this case, m m =(3.96-1)g*30wt%=0.89g.

[0043] The unloaded monomer solution can be recovered and reused.

[0044] (3) The swollen polyacrylonitrile powder is placed in a cobalt-60 irradiation field for radiation grafting polymerization, the radiation absorption dose is 8 kGy, the dose rate is 1 kGy / h, the irradiation temperature is room temperature, and the irradiation atmosphere is air.

[0045] (4) After the grafting polymerization was completed, the modified material was washed with hot water three times to remove a small amount of polymer on the surface, and then dried and weighed. The mass of the grafted polyacrylonitrile powder was 1.81 g. The grafting rate of the monomer on the material was calculated by the following formula:

[0046] Grafting rate (Degree of Grafting) = (m g -m0) / m0*100%, where m0,m g are the weights of the materials before and after grafting (g), respectively.

[0047] In this case, grafting rate = (1.81-1) g / 1 g*100% = 81%

[0048] The monomer utilization rate in the entire swelling grafting process is calculated by the following formula:

[0049] Utilization rate of monomer (URM) = (m g -m0) / mm *100%, where m m is the monomer loading after swelling (g), m0,m g are the weight of materials before and after grafting (g), respectively.

[0050] In this example, the monomer utilization ratio (URM) = (1.81-1) g / 0.89 g*100% = 91%.

[0051] Embodiment 2:

[0052] This embodiment provides a method for preparing a modified material based on polyacrylonitrile, comprising the following steps:

[0053] (1) Preparation of monomer solution: Prepare 10 mL of a mixed solution of N,N-dimethylformamide / water (1:2, v:v) containing methacrylic acid, with a final concentration of methacrylic acid of 35 wt %.

[0054] (2) 1 g of polyacrylonitrile powder (molecular weight M w 15×10 4 ) was placed in the prepared monomer solution and stirred at 40°C for 10 hours to swell. After the swelling was completed, the polyacrylonitrile powder was filtered from the monomer solution and weighed, with a mass of 3.60 g. The monomer loading m after the material swelled m =(3.60-1)g*35wt%=0.91g.

[0055] The unloaded monomer solution can be recovered and reused.

[0056] (3) The swollen polyacrylonitrile powder is placed in a cobalt-60 irradiation field for radiation grafting polymerization, the irradiation absorbed dose is 30 kGy, the dose rate is 1 kGy / h, the irradiation temperature is room temperature, and the irradiation atmosphere is nitrogen.

[0057] (4) After the grafting polymerization was completed, the modified material was washed three times with N,N-dimethylacetamide to remove a small amount of polymer on the surface, and then dried and weighed. The mass of the grafted material was 1.85 g, and the calculated monomer grafting rate was (1.85-1) g / 1 g*100%=85%.

[0058] During the entire swelling grafting process, the monomer utilization ratio (URM) = (1.85-1) g / 0.91 g*100% = 93.4%.

[0059] Embodiment 3:

[0060] This embodiment provides a method for preparing a modified material based on polyacrylonitrile, comprising the following steps:

[0061] (1) Preparation of monomer solution: Prepare 10 mL of a mixed solution of N,N-dimethylformamide / water (1:1, v:v) containing acrylonitrile, with a final concentration of acrylonitrile of 40 wt %.

[0062] (2) 1 g of polyacrylonitrile fiber (molecular weight M w 30×10 4 ) was placed in the prepared monomer solution and allowed to stand at room temperature for 10 hours to swell. After the swelling was completed, the polyacrylonitrile fiber was filtered from the monomer solution and weighed, with a mass of 3.34 g. The monomer loading m after the material swelled m =(3.34-1)g*40wt%=0.936g.

[0063] The unloaded monomer solution can be recovered and reused.

[0064] (3) The swollen polyacrylonitrile fiber is placed in an electron beam irradiation field for radiation grafting polymerization reaction, the irradiation absorbed dose is 50 kGy, the dose rate is 1 kGy / s, the irradiation temperature is room temperature, and the irradiation atmosphere is air.

[0065] (4) After the grafting polymerization was completed, the modified material was washed with N,N-dimethylformamide three times to remove a small amount of polymer on the surface, and then dried and weighed. The mass of the grafted material was 1.90 g, and the calculated monomer grafting rate = (1.90-1) g / 1 g*100% = 90%.

[0066] During the entire swelling grafting process, the monomer utilization ratio (URM) = (1.90-1) g / 0.936 g*100% = 96.2%.

[0067] (5) The modified material was subjected to amidoximation treatment. 1 g of the modified material was weighed and placed in a 10 wt% hydroxylamine hydrochloride methanol / water (1 / 1, v:v) mixed solution. The solution was adjusted to a pH of 7.0 with KOH in advance and reacted at 60° C. for 8 h. After the reaction was completed, the modified material was washed three times with deionized water and dried to obtain a modified material with amidoxime groups.

[0068] like Figure 1 The following are SEM images of polyacrylonitrile fiber, grafted polymer fiber, and amine oxime modified fiber. It can be seen that the diameter of the fiber becomes larger after swelling and grafting.

[0069] Embodiment 4:

[0070] This embodiment provides a method for preparing a modified material based on polyacrylonitrile, comprising the following steps:

[0071] (1) Preparation of monomer solution: Prepare 10 mL of benzene solution containing styrene, with a final styrene concentration of 40 wt %.

[0072] (2) 1 g of polyacrylonitrile particles (molecular weight M w 50×10 4 ) was placed in the prepared monomer solution and stirred at 60°C for 24 hours to swell. After swelling, the polyacrylonitrile particles were filtered from the monomer solution and weighed to a mass of 2.86 g. The monomer loading m after swelling of the material m =(2.86-1)g*40wt%=0.744g.

[0073] The unloaded monomer solution can be recovered and reused.

[0074] (3) The swollen polyacrylonitrile particles are placed in an electron beam irradiation field for radiation grafting polymerization reaction, the irradiation absorbed dose is 100 kGy, the dose rate is 1 kGy / s, the irradiation temperature is room temperature, and the irradiation atmosphere is air.

[0075] (4) After the grafting polymerization is completed, the modified material is washed with ethanol three times to remove a small amount of polymer on the surface, and then dried and weighed. The mass of the grafted material is 1.70 g, and the calculated monomer grafting rate = (1.70-1) g / 1 g*100% = 70%.

[0076] During the entire swelling grafting process, the monomer utilization ratio (URM) = (1.70-1) g / 0.744 g*100% = 94.0%.

[0077] (5) Weigh 1 g of the modified material, place it in a chloroform solution, and add concentrated sulfuric acid with a final concentration of 70% at 70°C while stirring for 5 hours to perform sulfonation treatment. After the reaction is completed, wash it three times with deionized water and dry it to obtain a modified material with sulfonic acid group ion exchange.

[0078] Embodiment 5:

[0079] This embodiment provides a method for preparing a modified material based on polyacrylonitrile, comprising the following steps:

[0080] (1) Preparation of monomer solution: Prepare 10 mL of chloroform solution containing 4-chloromethylstyrene, and the final concentration of 4-chloromethylstyrene is 40 wt %.

[0081] (2) 1 g of super polyacrylonitrile nonwoven fabric (molecular weight M w 50×10 4 ) was placed in the prepared monomer solution and stirred at room temperature for 24 hours to swell. After the swelling was completed, the polyacrylonitrile nonwoven fabric was filtered from the monomer solution and weighed, with a mass of 3.98 g. The monomer loading m after the material swelled m =(3.98-1)g*40wt%=1.192g.

[0082] The unloaded monomer solution can be recovered and reused.

[0083] (3) The swollen polyacrylonitrile nonwoven fabric is placed in an electron beam irradiation field for radiation graft polymerization reaction, the irradiation absorbed dose is 300 kGy, the dose rate is 2 kGy / s, the irradiation temperature is room temperature, and the irradiation atmosphere is air.

[0084] (4) After the grafting polymerization was completed, the modified material was washed with methanol three times to remove a small amount of polymer on the surface, and then dried and weighed. The mass of the grafted material was 2.11 g, and the calculated monomer grafting rate = (2.11-1) g / 1 g*100% = 111%.

[0085] During the entire swelling grafting process, the monomer utilization rate (URM) = (2.11-1) g / 1.192 g*100% = 93.1%.

[0086] (5) 1 g of the modified material was placed in 100 mL of a dimethyl sulfoxide solution containing triethylamine, the final concentration of triethylamine being 40 wt%, and reacted at 60° C. for 6 h. After the reaction was completed, the modified material was washed three times with deionized water and dried to obtain a quaternary ammonium ion exchange modified material.

[0087] Embodiment 6:

[0088] This embodiment provides a method for preparing a modified material based on polyacrylonitrile, comprising the following steps:

[0089] (1) Preparation of monomer solution: Prepare 10 mL of ethyl acetate solution containing glycidyl methacrylate, and the final concentration of glycidyl methacrylate is 35 wt %.

[0090] (2) 1 g of polyacrylonitrile powder (molecular weight M w 100×10 4 ) was placed in the prepared monomer solution and stirred at 60°C for 24 hours to swell. After the swelling was completed, the polyacrylonitrile powder was filtered from the monomer solution and weighed, with a mass of 4.02 g. The monomer loading m after the material swelled m =(4.02-1)g*35wt%=1.057g.

[0091] The unloaded monomer solution can be recovered and reused.

[0092] (3) The swollen polyacrylonitrile powder is placed in a cobalt-60 irradiation field for radiation grafting polymerization, the irradiation absorbed dose is 300 kGy, the dose rate is 5 kGy / h, the irradiation temperature is room temperature, and the irradiation atmosphere is nitrogen.

[0093] (4) After the grafting polymerization was completed, the modified material was washed with ethyl acetate three times to remove a small amount of polymer on the surface, and then dried and weighed. The mass of the grafted material was 2.01 g, and the monomer grafting rate was calculated as (2.01-1) g / 1 g*100%=101%.

[0094] During the entire swelling grafting process, the monomer utilization rate (URM) = (2.01-1) g / 1.057 g*100% = 95.6%.

[0095] (5) The modified materials are subjected to the following ring-opening reactions:

[0096] (5-1) The modified material is immersed in an isopropanol solution containing 70 wt % of amine small molecules such as ethylenediamine, diethylamine, diethyltriamine, or triethyltetramine, and reacted at 60° C. for 6 h to open the ring of glycidyl methacrylate and convert the epoxy group into an amino group, thereby obtaining a modified material with an amino group.

[0097] (5-2) The modified material is immersed in a solution containing 80% phosphoric acid and reacted at 80° C. for 6 h, so that the glycidyl methacrylate is ring-opened and the epoxy group is converted into a phosphoric acid group, thereby obtaining a modified material with a phosphoric acid group.

[0098] (5-3) The modified material is immersed in a 60% sodium sulfite solution and reacted at 60° C. for 8 h, so that the glycidyl methacrylate is ring-opened and the epoxy group is converted into a sulfonic acid group, thereby obtaining a modified material with a sulfonic acid group.

[0099] Embodiment 7:

[0100] This embodiment provides a method for preparing a modified material based on polyacrylonitrile, comprising the following steps:

[0101] (1) Preparation of monomer solution: Prepare 10 mL of a methanol solution containing 4-hydroxybutyl acrylate glycidyl ether, wherein the final concentration of 4-hydroxybutyl acrylate glycidyl ether is 40 wt %.

[0102] (2) 1 g of polyacrylonitrile powder (molecular weight M w 150×10 4 ) was placed in the prepared monomer solution and stirred at 60°C for 24 hours to swell. After the swelling was completed, the polyacrylonitrile powder was filtered from the monomer solution and weighed, with a mass of 4.36 g. The monomer loading m after the material swelled m =(4.36-1)g*40wt%=1.344g.

[0103] The unloaded monomer solution can be recovered and reused.

[0104] (3) placing the swollen polyacrylonitrile powder in a cobalt-60 irradiation field for radiation grafting polymerization, with an absorbed irradiation dose of 150 kGy, a dose rate of 5 kGy / h, an irradiation temperature of room temperature, and an irradiation atmosphere of nitrogen.

[0105] (4) After the grafting polymerization was completed, the modified material was washed with ethyl acetate three times to remove a small amount of polymer on the surface, and then dried and weighed. The mass of the grafted material was 2.24 g, and the calculated monomer grafting rate = (2.24-1) g / 1 g*100% = 124%.

[0106] During the entire swelling grafting process, the monomer utilization ratio (URM) = (2.24-1) g / 1.344 g*100% = 92.3%.

[0107] (5) The modified materials are subjected to the following ring-opening reactions:

[0108] (5-1) The modified material is immersed in an isopropanol solution containing 70 wt % of ethylenediamine or diethylamine or diethyltriamine or triethyltetramine, and reacted at 60° C. for 6 h, so that the glycidyl methacrylate is ring-opened and the epoxy group is converted into an amino group, thereby obtaining a modified material with an amino group.

[0109] (5-2) The modified material is immersed in a solution containing 80% phosphoric acid and reacted at 80° C. for 6 hours, so that the glycidyl methacrylate is ring-opened and the epoxy group is converted into a phosphoric acid group, thereby obtaining a modified material with a phosphoric acid group.

[0110] (5-3) The modified material is immersed in a 60% sodium sulfite solution and reacted at 60° C. for 8 h, so that the glycidyl methacrylate is ring-opened and the epoxy group is converted into a sulfonic acid group, thereby obtaining a modified material with a sulfonic acid group.

[0111] Embodiment 8:

[0112] This embodiment provides a method for preparing a modified material based on polyacrylonitrile, comprising the following steps:

[0113] (1) Preparation of monomer solution: Prepare 10 mL of dimethyl sulfoxide solution containing hydroxyethyl acrylate, and the final concentration of hydroxyethyl acrylate is 40 wt %.

[0114] (2) 1 g of polyacrylonitrile fiber (molecular weight M w 50×10 4 ) was placed in the prepared monomer solution and stirred at 40°C for 24 hours to swell. After swelling, the polyacrylonitrile fiber was filtered from the monomer solution and weighed, with a mass of 4.58 g. The monomer loading m after swelling of the material m =(4.58-1)g*40wt%=1.432g.

[0115] The unloaded monomer solution can be recovered and reused.

[0116] (3) The swollen polyacrylonitrile fiber is placed in an electron beam irradiation field for radiation grafting polymerization reaction, the irradiation absorbed dose is 50 kGy, the dose rate is 1 kGy / s, the irradiation temperature is room temperature, and the irradiation atmosphere is air.

[0117] (4) After the grafting polymerization was completed, the modified material was washed with dimethyl sulfoxide three times to remove a small amount of polymer on the surface, and then dried and weighed. The mass of the grafted material was 2.36 g, and the calculated monomer grafting rate = (2.36-1) g / 1 g*100% = 136%.

[0118] During the entire swelling grafting process, the monomer utilization ratio (URM) = (2.36-1) g / 1.432 g*100% = 95.0%.

[0119] (5) The grafted material can be further modified by conventional methods.

[0120] Embodiment 9:

[0121] This embodiment provides a method for preparing a modified material based on polyacrylonitrile, comprising the following steps:

[0122] (1) Preparation of monomer solution: Prepare 10 mL of ethanol solution containing vinylaniline, and the final concentration of vinylaniline is 10 wt %.

[0123] (2) 1 g of polyacrylonitrile nonwoven fabric (molecular weight M w 50×10 4 ) was placed in the prepared monomer solution and stirred at room temperature for 24 hours to swell. After the swelling was completed, the polyacrylonitrile nonwoven fabric was filtered from the monomer solution and weighed, with a mass of 2.97 g. The monomer loading m after the material swelled m =(2.97-1)g*10wt%=0.197g.

[0124] The unloaded monomer solution can be recovered and reused.

[0125] (3) placing the swollen polyacrylonitrile nonwoven fabric in an electron beam irradiation field for radiation graft polymerization, with an absorbed irradiation dose of 200 kGy, a dose rate of 1 kGy / s, an irradiation temperature of room temperature, and a vacuum atmosphere.

[0126] (4) After the grafting polymerization was completed, the modified material was washed with ethanol three times to remove a small amount of polymer on the surface, and then dried and weighed. The mass of the grafted material was 1.18 g, and the calculated monomer grafting rate = (1.18-1) g / 1 g*100% = 18%.

[0127] During the entire swelling grafting process, the monomer utilization rate (URM) = (1.18-1) g / 0.197 g*100% = 91.3%.

[0128] (5) The above 0.2 g modified material was placed in 40 mL of hydrochloric acid solution with a pH of 1.5, and 10 mL of 1 mol / L aniline solution and 10 mL of 1 mol / L ammonium persulfate solution were added dropwise at a rate of 2.5 mL / h for 4 times. The mixture was reacted in an ice bath for 24 h. After the reaction was completed, the mixture was washed three times with deionized water and dried to obtain a polyaniline-modified photothermal conversion material.

[0129] Embodiment 10:

[0130] This embodiment provides a method for preparing a modified material based on polyacrylonitrile, comprising the following steps:

[0131] (1) Preparation of monomer solution: Prepare 10 mL of ethanol solution containing vinyl pyrrole, and the final concentration of vinyl pyrrole is 10 wt %.

[0132] (2) 1 g of polyacrylonitrile nonwoven fabric (molecular weight M w 50×10 4 ) was placed in the prepared monomer solution and stirred at room temperature for 24 hours to swell. After the swelling was completed, the polyacrylonitrile nonwoven fabric was filtered from the monomer solution and weighed, with a mass of 2.33 g. The monomer loading m after the material swelled m =(2.33-1)g*10wt%=0.133g.

[0133] The unloaded monomer solution can be recovered and reused.

[0134] (3) placing the swollen polyacrylonitrile nonwoven fabric in an electron beam irradiation field for radiation graft polymerization reaction, the irradiation absorbed dose is 200 kGy, the dose rate is 1 kGy / s, the irradiation temperature is room temperature, and the irradiation atmosphere is vacuum.

[0135] (4) After the grafting polymerization was completed, the modified material was washed with ethanol three times to remove a small amount of polymer on the surface, and then dried and weighed. The mass of the grafted material was 1.12 g, and the calculated monomer grafting rate was (1.12-1) g / 1 g*100%=12%.

[0136] During the entire swelling grafting process, the monomer utilization ratio (URM) = (1.12-1) g / 0.133 g*100% = 90.2%.

[0137] (5) 1 g of the modified material was placed in a sulfuric acid-adjusted aqueous solution with a pH of 1, 6 g of FeCl3 was added, and the mixture was stirred at room temperature for 1 h. 1.25 g of pyrrole was added, and the reaction was continued in an ice bath (<10° C.) for 6 hours to obtain a polypyrrole-modified photothermal conversion material.

[0138] Embodiment 11:

[0139] This embodiment provides a method for preparing a modified material based on polyacrylonitrile, comprising the following steps:

[0140] (1) Preparation of monomer solution: Prepare 10 mL of an aqueous solution containing polyvinyl alcohol, with a final concentration of polyvinyl alcohol of 15 wt %.

[0141] (2) 1 g of polyacrylonitrile film (molecular weight M) w 30×10 4 ) was placed in the prepared monomer solution and stirred at 60°C for 24 hours to swell. After the swelling was completed, the polyacrylonitrile film was filtered from the monomer solution and weighed, with a mass of 2.84 g. The monomer loading m after the material swelled m =(2.84-1)g*15wt%=0.276g.

[0142] The unloaded monomer solution can be recovered and reused.

[0143] (3) The swollen polyacrylonitrile film is placed in an electron beam irradiation field for radiation graft polymerization reaction, the irradiation absorbed dose is 50 kGy, the dose rate is 1 kGy / s, the irradiation temperature is room temperature, and the irradiation atmosphere is air.

[0144] (4) After the grafting polymerization was completed, the modified material was washed with water three times to remove a small amount of polymer on the surface, and then dried and weighed. The mass of the grafted material was 1.26 g, and the calculated monomer grafting rate was (1.26-1) g / 1 g*100%=26%.

[0145] During the entire swelling grafting process, the monomer utilization ratio (URM) = (1.26-1) g / 0.276 g*100% = 94.2%.

[0146] After grafting modification, the hydrophilicity of polyacrylonitrile film was improved and the water contact angle was reduced to 35°.

[0147] Embodiment 12:

[0148] This embodiment provides a method for preparing a modified material based on polyacrylonitrile, comprising the following steps:

[0149] (1) Preparation of monomer solution: Prepare 10 mL of aqueous solution containing polyacrylamide, with a final concentration of polyacrylamide of 10 wt %.

[0150] (2) 1 g of polyacrylonitrile nonwoven fabric (molecular weight M w 30×10 4) was placed in the prepared monomer solution and stirred at 60°C for 24 hours to swell. After the swelling was completed, the polyacrylonitrile nonwoven fabric was filtered from the monomer solution and weighed, with a mass of 2.65 g. The monomer loading m after the material swelled m =(2.65-1)g*10wt%=0.165g.

[0151] The unloaded monomer solution can be recovered and reused.

[0152] (3) The swollen polyacrylonitrile nonwoven fabric is placed in an electron beam irradiation field for radiation graft polymerization reaction, the irradiation absorbed dose is 50 kGy, the dose rate is 1 kGy / s, the irradiation temperature is room temperature, and the irradiation atmosphere is air.

[0153] (4) After the grafting polymerization was completed, the modified material was washed with water three times to remove a small amount of polymer on the surface, and then dried and weighed. The mass of the grafted material was 1.15 g, and the calculated monomer grafting rate = (1.15-1) g / 1 g*100% = 15%.

[0154] During the entire swelling grafting process, the monomer utilization ratio (URM) = (1.15-1) g / 0.165 g*100% = 90.9%.

[0155] After grafting modification, the hydrophilicity of polyacrylonitrile nonwoven fabric is improved, and the water contact angle is reduced to 38°.

[0156] Embodiment 13:

[0157] This embodiment provides a method for preparing a modified material based on polyacrylonitrile, comprising the following steps:

[0158] (1) Preparation of monomer solution: Prepare 10 mL of aqueous solution containing acrylamide, with a final concentration of acrylamide of 40 wt %.

[0159] (2) 1 g of polyacrylonitrile nonwoven fabric (molecular weight M w 30×10 4 ) was placed in the prepared monomer solution and stirred at 60°C for 24 hours to swell. After the swelling was completed, the polyacrylonitrile nonwoven fabric was filtered from the monomer solution and weighed, with a mass of 3.77 g. The monomer loading m after the material swelled m =(3.77-1)g*40wt%=1.108g.

[0160] The unloaded monomer solution can be recovered and reused.

[0161] (3) The swollen polyacrylonitrile nonwoven fabric is placed in an electron beam irradiation field for radiation graft polymerization reaction, the irradiation absorbed dose is 50 kGy, the dose rate is 1 kGy / s, the irradiation temperature is room temperature, and the irradiation atmosphere is air.

[0162] (4) After the grafting polymerization was completed, the modified material was washed with water three times to remove a small amount of polymer on the surface, and then dried and weighed. The mass of the grafted material was 2.04 g, and the calculated monomer grafting rate = (2.04-1) g / 1 g*100% = 104%.

[0163] During the entire swelling grafting process, the monomer utilization ratio (URM) = (2.04-1) g / 1.108 g*100% = 93.9%.

[0164] After grafting modification, the hydrophilicity of polyacrylonitrile nonwoven fabric is improved, and the water contact angle is reduced to 38°.

[0165] The modified materials in the above-mentioned embodiments 1-13, materials with chelating functions such as hydroxyl groups (embodiments 1, 2, 6, 7, 11), amine groups (embodiments 6, 7, 12, 13), amidoxime groups (embodiment 3), and materials with ion exchange capacity such as carboxylic acid groups (embodiments 1, 2), quaternary amine groups (embodiments 5, 6, 7), sulfonic acid groups (embodiments 4, 6, 7), and phosphoric acid groups (embodiments 6, 7) can be applied to the adsorption and separation of metal ions;

[0166] The modified material with polyaniline conductive polymer in Example 9 and the modified material with polypyrrole conductive polymer in Example 10 can be applied to photothermal conversion materials.

[0167] Each modified final product material was placed in a solution containing different metal ions for adsorption and separation, and the adsorption capacity and adsorption rate were calculated based on the difference in the concentration of each ion in the solution and the mass of the input material, as shown in Table 1 below; Table 1 Adsorption capacity and adsorption rate of the modified final products prepared in Examples 1-8 in metal ion solutions

[0168]

[0169]

[0170] The 2 cm*2 cm modified materials prepared in Examples 9 and 10 were placed in 50 mL of aqueous solution and irradiated at an intensity of 1 sun to obtain the water evaporation performance shown in Table 2:

[0171] Table 2. Water evaporation performance of the modified final products prepared in Examples 9 and 10 of the present invention

[0172]

[0173] Comparative Example 1:

[0174] (1) Preparation of monomer solution: Prepare 200 mL of a mixed solution of N,N-dimethylformamide / water (1:1, v:v) containing acrylic acid, the final concentration of acrylic acid being 10 wt%. The amount of monomer added is 20 g.

[0175] (2) 1 g of polyacrylonitrile powder (molecular weight M w 8×10 4 ) is placed in the prepared monomer solution and placed in a cobalt-60 irradiation field for radiation grafting polymerization reaction, the irradiation absorbed dose is 8 kGy, the dose rate is 1 kGy / h, the irradiation temperature is room temperature, and the irradiation atmosphere is air.

[0176] (4) After the grafting polymerization was completed, the modified material was washed with hot water three times to remove a small amount of polymer on the surface, and then dried and weighed. The mass of the grafted material was 1.63 g, and the calculated monomer grafting rate = (1.63-1) g / 1 g*100% = 63%.

[0177] During the whole grafting process, the monomer utilization rate (URM) = (1.63-1) g / 20 g*100% = 3.15%.

[0178] In this comparative example 1, the swelling step is omitted, and the monomer utilization rate for grafting acrylic acid onto polyacrylonitrile powder is low, requiring a large amount of monomer solution to induce grafting. In this comparative example, 200 mL of monomer solution, the monomer utilization rate is only 3.15%.

[0179] In addition, a large amount of polyacrylic acid homopolymer also appeared in the 200 mL monomer solution in Comparative Example 1, and the polyacrylonitrile powder was mixed with the homopolymer and was difficult to separate.

[0180] Comparative Example 2:

[0181] (1) Preparation of monomer solution: 100 mL of aqueous solution containing acrylamide was prepared, the final concentration of acrylamide was 10 wt %, and the added mass of acrylamide monomer was 10 g.

[0182] (2) 1 g of polyacrylonitrile nonwoven fabric (molecular weight M w 15×10 4 ) is placed in the prepared monomer solution and placed in an electron beam irradiation field for radiation grafting polymerization reaction, the irradiation absorbed dose is 50 kGy, the dose rate is 1 kGy / s, the irradiation temperature is room temperature, and the irradiation atmosphere is air.

[0183] (4) After the grafting polymerization was completed, the modified material was washed with water three times to remove a small amount of polymer on the surface, and then dried and weighed. The mass of the grafted material was 1.46 g, and the calculated monomer grafting rate = (1.46-1) g / 1 g*100% = 46%.

[0184] During the entire grafting process, the monomer utilization rate (URM) = (1.46-1) g / 10 g*100% = 4.6%.

[0185] In this comparative example 2, the swelling step is omitted, and the monomer utilization rate for grafting acrylamide on polyacrylonitrile nonwoven fabric is low, and a large amount of monomer solution is required to induce grafting. In this comparative example, 100 mL of monomer solution has a monomer utilization rate of only 4.6%.

[0186] In addition, a large amount of acrylic acid homopolymer also appeared in the 100 mL monomer solution in Comparative Example 2, and the polyacrylonitrile nonwoven fabric was mixed with the homopolymer and was difficult to separate.

[0187] Comparative Example 3:

[0188] (1) Preparation of monomer solution: Prepare 100 mL of N,N-dimethylformamide solution containing acrylonitrile monomer, the final concentration of acrylonitrile is 40 wt %, and the added mass of acrylamide monomer is 40 g.

[0189] (2) 1 g of polyacrylonitrile fiber (molecular weight M w 50×10 4 ) is placed in the prepared monomer solution and placed in an electron beam irradiation field for radiation grafting polymerization reaction, the irradiation absorbed dose is 50 kGy, the dose rate is 1 kGy / s, the irradiation temperature is room temperature, and the irradiation atmosphere is air.

[0190] (4) After the grafting polymerization was completed, the modified material was washed with water three times to remove a small amount of polymer on the surface, and then dried and weighed. The mass of the grafted material was 2.13 g, and the calculated monomer grafting rate = (2.13-1) g / 1 g*100% = 113%.

[0191] During the whole grafting process, the monomer utilization ratio (URM) = (2.13-1) g / 40 g*100% = 2.8%.

[0192] In this comparative example 2, the swelling step is omitted, and the monomer utilization rate for grafting acrylonitrile on polyacrylonitrile fiber is low, and a large amount of monomer solution is required to induce grafting. In this comparative example, 100 mL of monomer solution has a monomer utilization rate of only 2.8%.

[0193] In addition, a large amount of acrylic acid homopolymer also appeared in the 100 mL monomer solution in Comparative Example 2, and the polyacrylonitrile fiber was mixed with the homopolymer and was difficult to separate.

[0194] The present invention utilizes polyacrylonitrile for grafting in a swollen state, and the swelling allows the monomer solution to enter the interior of the polymer substrate in advance, thereby reducing the monomer diffusion resistance in the traditional radiation grafting process, achieving high monomer utilization and grafting efficiency.

[0195] Even if the monomer loading rate of the polyacrylonitrile solid material is low, such as 10-40% in the above embodiment, the mass of the monomer solution carried on the material is 10-40% of the mass used when preparing the solution, and the monomers in the monomer solution can be efficiently utilized, and the unused monomers are not in contact with the radiation rays and can be recycled and reused. However, in the prior art, due to the low utilization rate of pre-irradiation grafting or traditional co-irradiation grafting monomers (Nucl. Sci. Tech. 2019, 30 (2): 20.; Ind. Eng. Chem. Res., 2016, 55, (15), 4118-4124), a large amount of monomer capacity needs to be configured to disperse the substrate therein to induce grafting. The mass of the monomer solution is usually more than 100 times the mass of the solid substrate. And once the monomer solution configured with 100 times the mass of the substrate is used, it is difficult to recycle. The amount of monomer solution used in the present invention is reduced by 50-200 times compared with traditional graft polymerization, and the monomer utilization rate is increased by 30 times, which is more economical.

[0196] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A method for preparing a modified material based on polyacrylonitrile, characterized in that: The steps include: S1, soaking polyacrylonitrile in a solution containing a grafting monomer to swell; S2. Irradiate the polyacrylonitrile that has been swollen in step S1 to initiate a graft polymerization reaction of the monomers, thereby obtaining a modified material based on polyacrylonitrile.

2. The method for preparing a modified material based on polyacrylonitrile according to claim 1, characterized in that: In step S1, the molecular weight of the polyacrylonitrile is M w (8-300)×10 4 .

3. The method for preparing a modified material based on polyacrylonitrile according to claim 1, characterized in that: In step S1, the final concentration of the grafting monomer in the solution is 10wt%-40wt%; The grafting monomer is selected from any one or more of acrylic acid, methacrylic acid, acrylonitrile, styrene, 4-chloromethylstyrene, glycidyl methacrylate, 4-hydroxybutyl acrylate glycidyl ether, hydroxyethyl acrylate, vinyl aniline, vinyl pyrrole, polyvinyl alcohol, and polyacrylamide; The solution is selected from any one or more of methanol, ethanol, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, ethyl acetate, acetone, benzene, chloroform and water.

4. The method for preparing a modified material based on polyacrylonitrile according to claim 1, characterized in that: In step S1, the swelling time is 4-48 hours, the swelling temperature is 10-60° C., and the swelling method is stirring swelling or static swelling.

5. The method for preparing a modified material based on polyacrylonitrile according to claim 1, characterized in that: In step S2, the irradiation source used for irradiation is an electron accelerator or cobalt-60, and the irradiation method is co-irradiation.

6. The method for preparing a modified material based on polyacrylonitrile according to claim 5, characterized in that: When the radiation source is an electron accelerator, the radiation dose rate is 1-5 kGy / s; when the radiation source is cobalt-60, the radiation dose rate is 1-5 kGy / h.

7. The method for preparing a modified material based on polyacrylonitrile according to claim 1, characterized in that: In step S2, the irradiation absorbed dose is 5-300 kGy, the irradiation temperature is room temperature, and the irradiation atmosphere is air, nitrogen or vacuum atmosphere.

8. A modified material based on polyacrylonitrile, characterized in that: Obtained based on the preparation method described in any one of claims 1-7.

9. An application of the modified material based on polyacrylonitrile as claimed in claim 8, characterized in that: The modified material based on polyacrylonitrile is used as an adsorption material and / or a light-to-heat conversion material.

10. The use of the modified material based on polyacrylonitrile according to claim 9, characterized in that: The adsorption material and the photothermal conversion material are obtained by post-processing the modified material based on polyacrylonitrile: When the modified material based on polyacrylonitrile has an epoxy group, a ring-opening reaction is performed; When the polyacrylonitrile-based modified material has a cyano group, an oximation reaction is performed; When the modified material based on polyacrylonitrile has a chlorophenyl group, a sulfonation reaction and / or a quaternization reaction is performed; Alternatively, aniline is added to the modified material based on polyacrylonitrile to perform a polyaniline modification reaction or pyrrole is added to perform a polypyrrole modification reaction.

Citation Information

Patent Citations

  • Preparation method of polyacrylonitrile adsorbing materials

    CN101899132A

  • High-polymer material functional modification

    CN1817943A

  • Process for preparing acrylonitrile graft polymers

    DE1720632A1

  • Manufacture of grafted polymers

    US2983657A

Cited By

  • Anti-interference control cable

    CN119418993A

  • Anti-interference control cable

    CN119418993B

  • Weather-resistant anti-aging polypropylene material and preparation method thereof

    CN120310136A