Liquid crystal polymer, fiber and preparation method and application thereof
The preparation of liquid crystal polymer fibers through a specific ratio of liquid crystal polymer monomers solves the problems of surface peeling and lowering of friction coefficient of the transmission belt, and achieves high wear resistance and suitable friction coefficient of the liquid crystal polymer fibers, meeting the application needs of the transmission belt.
Patent Information
- Application Number
- CN202411190605.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-12
AI Technical Summary
During use, the transmission belt is prone to surface peeling, wear and reduced friction coefficient problems, which affects its wear resistance and load bearing capacity.
The liquid crystal polymer monomer with a specific ratio is prepared by prepolymerization and solid phase polycondensation reaction, and fibers are prepared by spinning process, combining suitable catalysts and extrusion temperatures to obtain good spinning and wear resistance. liquid crystal polymer fiber.
The obtained liquid crystal polymer fiber not only has better wear resistance, but also has an appropriate friction coefficient, which fully meets the application requirements of the transmission belt, extends the service life and improves the performance of the transmission belt.
Smart Images

Figure CN118930828A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer materials, and in particular relates to a liquid crystal polymer, fiber, and a preparation method and application thereof. Background Art
[0002] The transmission belt is used to transmit the power generated by the rotation of the motor or engine of the prime mover to the mechanical equipment through the pulley. It can freely change speed, transmit long and short distances, and has a simple, economical structure and is easy to use. It has a wide range of uses, including electric motors, agricultural machinery, machine tools, automobiles, ships, air transportation, household appliances, office equipment and other fields. It can be said that belts will be used wherever there is power output. However, as the use becomes more and more extensive, more problems have also emerged during use, such as wear, scratches, ruptures, difficulty in cleaning, and difficulty in recycling.
[0003] At present, transmission belts are mostly made of polymer materials such as PVC, rubber, nylon, etc. As we all know, during the use of the transmission belt, its surface will contact the object being transmitted, and the friction generated by the contact between the surface of the transmission belt and the object is used to transport the object. During the use of the transmission belt, its surface is in contact with the object for a long time, and it will be peeled off by the object being transported above. After the transmission belt has been used for a period of time, the surface of the transmission belt is prone to peeling off from the transmission belt, causing it to fall off, affecting the normal use of the transmission belt. Therefore, in order to further extend the application field of the transmission belt and further extend its service life, its wear resistance still needs to be improved.
[0004] In order to improve the wear resistance of polymer materials in the prior art, the materials are generally modified by adding wear-resistant agents, which include liquid silicone, graphite, PTFE, molybdenum disulfide, etc. Most wear-resistant agents, whether powder or liquid, will migrate to the surface of the material, thereby reducing the surface friction coefficient of the material and improving the wear resistance of the material. Although the above method can improve the wear resistance of the material, it also reduces the friction coefficient of the material surface. For the transmission belt, the reduction of the friction coefficient means a decrease in its load-bearing capacity, which also affects normal use. Summary of the invention
[0005] The object of the present invention is to provide a liquid crystal polymer material with good spinnability in view of the above technical problems. The fiber made of the liquid crystal polymer material has good wear resistance and a moderate friction coefficient and can be used for transmission belts.
[0006] The technical solution adopted by the present invention to solve the above technical problem is: a method for preparing a liquid crystal polymer, which comprises the following preparation steps:
[0007] A1: mixing monomers p-hydroxybenzoic acid, 1,1'-bi-2-naphthol, terephthalic acid with an acylating agent and a catalyst to obtain a reaction mixture; wherein, by mole, the mole fractions of the three monomers are as follows: 100 parts of p-hydroxybenzoic acid, 5-15 parts of 1,1'-bi-2-naphthol, and 3-10 parts of terephthalic acid;
[0008] A2: subjecting the reaction mixture to a prepolymerization reaction to obtain a prepolymer;
[0009] A3: Under an inert gas atmosphere, subjecting the prepolymer to a solid phase polycondensation reaction to obtain a polycondensate;
[0010] A4: The obtained polycondensate is mixed with 2-5 mole parts of 2,5-bipyridinecarboxylic acid in a screw extruder and extruded to obtain a liquid crystal polymer.
[0011] Preferably, the sum of the molar fractions of terephthalic acid and 2,5-bipyridinecarboxylic acid is equal to the molar fraction of 1,1'-bi-2-naphthol.
[0012] Preferably, the catalyst is 2-(4-methylpiperazine)-3-aminopyridine, and the added amount is 400-500 ppm of the total weight of the three monomers of p-hydroxybenzoic acid, 1,1'-bi-2-naphthol and terephthalic acid.
[0013] Preferably, in step A4, the extrusion temperature of the screw extruder is 300-330°C.
[0014] The second object of the present invention is to provide a liquid crystal polymer, which is prepared by the above-mentioned method for preparing a liquid crystal polymer.
[0015] The third object of the present invention is to provide a method for preparing liquid crystal polymer fibers, the method comprising the following steps:
[0016] a1: heating and extruding the liquid crystal polymer as described above, supplying the polymer to a spinning assembly, ejecting fiber filaments through the spinning assembly, and subjecting the fiber filaments to heat preservation, air cooling, drawing and shaping, and filament separation and winding to obtain nascent fibers;
[0017] a2: heat-treating the spun fibers to obtain finished fibers.
[0018] Preferably, the insulation temperature in step a1 is 280-300° C., and the speed of the stretching and shaping is 800-900 m / min.
[0019] Preferably, the heat treatment temperature in step a2 is 280-330° C. and the time is 12-24 hours.
[0020] The present invention also provides a liquid crystal polymer fiber, which is prepared by the above-mentioned preparation method of the liquid crystal polymer fiber.
[0021] Another object of the present invention is to provide an application of the liquid crystal polymer fiber in a transmission belt.
[0022] The beneficial technical effects of the present invention are:
[0023] The liquid crystal polymer obtained by the invention using a specific ratio of polymerization monomers and catalysts and a special preparation process has better spinnability and appearance. The finished fiber obtained by the spinning process has not only good wear resistance but also a suitable friction coefficient, which fully meets the application requirements of the transmission belt. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 : Appearance diagram of the finished fiber wear resistance test in Example 1;
[0025] Figure 2 : Appearance of the finished fiber wear resistance test in Comparative Example 2. DETAILED DESCRIPTION
[0026] In order to make the above-mentioned objects, features and advantages of the present invention more clearly understood, the specific embodiments of the present invention are described in detail below. Unless otherwise specified, materials, equipment and reagents are all commercially available.
[0027] An embodiment of the present invention provides a method for preparing a liquid crystal polymer, comprising the following steps A1: mixing monomers p-hydroxybenzoic acid, 1,1'-bi-2-naphthol, and terephthalic acid with an acylating agent and a catalyst to obtain a reaction mixture; wherein, in terms of molar fractions, the molar fractions of the three monomers are as follows: 100 parts of p-hydroxybenzoic acid, 5-15 parts of 1,1'-bi-2-naphthol, and 3-10 parts of terephthalic acid;
[0028] A2: subjecting the reaction mixture to a prepolymerization reaction to obtain a prepolymer;
[0029] A3: Under an inert gas atmosphere, subjecting the prepolymer to a solid phase polycondensation reaction to obtain a polycondensate;
[0030] A4: The obtained polycondensate is mixed with 2-5 molar parts of 2,5-bipyridinecarboxylic acid in a screw extruder and extruded to obtain a liquid crystal polymer.
[0031] Optionally, the reaction mixture in step A2 is subjected to a prepolymerization reaction to obtain a prepolymer, comprising: keeping the reaction mixture at 130-150° C. for 1-3 h, then heating it to 290-330° C. and keeping it for 1-3 h, then filling a Hastelloy kettle with 0.2-1.0 MPa inert gas, discharging the reaction product through a discharge valve with a diameter of 2-4 mm and 8-10 holes, crushing it, passing it through a 20-30 mesh sieve, and drying it at 110-130° C. for 1-2 h to obtain the prepolymer.
[0032] Optionally, in step A3, the temperature of the solid phase polycondensation reaction is 280-330° C., and the time is 12-36 hours.
[0033] Optionally, in step A1, the catalyst is 2-(4-methylpiperazine)-3-aminopyridine, and the added amount is 400-500 ppm of the total weight of the three monomers of p-hydroxybenzoic acid, 1,1'-bi-2-naphthol and terephthalic acid.
[0034] Optionally, in step A1, the acylating agent is acetic anhydride, and the added amount is 1.05-1.6 times the total molar number of hydroxyl groups in the three monomers of p-hydroxybenzoic acid, 1,1'-bi-2-naphthol and terephthalic acid.
[0035] An embodiment of the present invention further provides a liquid crystal polymer, which is prepared by the above-mentioned preparation method of the liquid crystal polymer.
[0036] An embodiment of the present invention further provides a method for preparing a liquid crystal polymer fiber, which comprises the following steps:
[0037] a1: heating and extruding the liquid crystal polymer as claimed in claim 5, supplying the polymer to a spinning assembly, ejecting fiber filaments through the spinning assembly, and subjecting the fiber filaments to heat preservation, air cooling, drawing and shaping, and filament separation and winding to obtain nascent fibers;
[0038] a2: heat-treating the spun fibers to obtain finished fibers.
[0039] Optionally, in step a1, the liquid crystal polymer is heated to 300-330° C. and then extruded.
[0040] Optionally, the insulation temperature in step a1 is 280-300° C., and the speed of the drawing and shaping is 800-900 m / min.
[0041] Optionally, the heat treatment temperature in step a2 is 280-330° C. and the time is 12-24 hours.
[0042] An embodiment of the present invention further provides a liquid crystal polymer fiber, which is prepared by the above-mentioned preparation method of the liquid crystal polymer fiber.
[0043] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention.
[0044] Table 1 is a table of monomer ratios in Examples 1-4.
[0045] Table (1)
[0046]
[0047] Example 1
[0048] According to the 1# ratio, monomers p-hydroxybenzoic acid, 1,1'-bi-2-naphthol, terephthalic acid, acylating agent acetic anhydride accounting for 1.05 times the total molar number of hydroxyl groups of the three monomers, and catalyst 2-(4-methylpiperazine)-3-aminopyridine accounting for 400ppm of the total weight of the three monomers are put into a Hastelloy kettle and kept at 130°C for 3 hours, then the temperature is raised to 290°C and kept for 3 hours, and then 0.2MPa of inert gas is filled into the Hastelloy kettle, and the reaction product material is discharged through a discharge valve with a diameter of 4mm and 8 holes, crushed, passed through a 20-mesh sieve, and dried at 110°C for 1 hour to obtain the prepolymer; in an inert gas atmosphere, the prepolymer is subjected to solid phase polycondensation reaction at 280°C for 36 hours to obtain a polycondensate; the obtained polycondensate is mixed and extruded with 2,5-bipyridinecarboxylic acid at 300°C in a screw extruder with a rotation speed of 300r / min at 300°C to obtain a liquid crystal polymer.
[0049] The liquid crystal polymer is heated to 300°C and then extruded, supplied to a spinning assembly, through which fiber filaments are ejected, the fiber filaments are kept at 280°C for 5 minutes, then air-cooled to room temperature, and then stretched and shaped at a speed of 800m / min, and finally divided and wound to obtain spun fibers; the spun fibers are heat treated at 280°C for 24 hours to obtain finished fibers.
[0050] Example 2
[0051] According to the 1# ratio, monomers p-hydroxybenzoic acid, 1,1'-bi-2-naphthol, terephthalic acid, acylating agent acetic anhydride accounting for 1.2 times the total molar number of hydroxyl groups of the three monomers, and catalyst 2-(4-methylpiperazine)-3-aminopyridine accounting for 430 ppm of the total weight of the three monomers are put into a Hastelloy kettle and kept at 140°C for 2 hours, then the temperature is raised to 300°C and kept for 2 hours, and then 0.5 MPa of inert gas is filled into the Hastelloy kettle, and the reaction product material is discharged through a discharge valve with a diameter of 2 mm and 8 holes, crushed, passed through a 20-mesh sieve, and dried at 120°C for 2 hours to obtain the prepolymer; in an inert gas atmosphere, the prepolymer is subjected to solid phase polycondensation reaction at 290°C for 24 hours to obtain a polycondensate; the obtained polycondensate is mixed and extruded with 2,5-bipyridinecarboxylic acid at 310°C in a screw extruder with a rotation speed of 300 r / min to obtain a liquid crystal polymer.
[0052] The liquid crystal polymer is heated to 310°C and then extruded, supplied to a spinning assembly, through which fiber filaments are ejected, the fiber filaments are kept at 290°C for 5 minutes, then air-cooled to room temperature, and then stretched and shaped at a speed of 900 m / min, and finally divided and wound to obtain spun fibers; the spun fibers are heat treated at 300°C for 18 hours to obtain finished fibers.
[0053] Example 3
[0054] According to the 1# ratio, monomers p-hydroxybenzoic acid, 1,1'-bi-2-naphthol, terephthalic acid, acylating agent acetic anhydride accounting for 1.5 times the total molar number of hydroxyl groups of the three monomers, and catalyst 2-(4-methylpiperazine)-3-aminopyridine accounting for 460 ppm of the total weight of the three monomers are put into a Hastelloy kettle and kept at 140°C for 1 hour, then the temperature is raised to 310°C and kept for 3 hours, and then 0.8 MPa of inert gas is filled into the Hastelloy kettle, and the reaction product material is discharged through a discharge valve with a diameter of 4 mm and a number of holes of 10, crushed, passed through a 30-mesh sieve, and dried at 130°C for 1 hour to obtain the prepolymer; in an inert gas atmosphere, the prepolymer is subjected to solid phase polycondensation reaction at 310°C for 16 hours to obtain a polycondensate; the obtained polycondensate is mixed and extruded with 2,5-bipyridinecarboxylic acid at 320°C in a screw extruder with a rotation speed of 300 r / min to obtain a liquid crystal polymer.
[0055] The liquid crystal polymer is heated to 320°C and then extruded, supplied to a spinning assembly, through which fiber filaments are ejected, the fiber filaments are kept at 290°C for 5 minutes, then air-cooled to room temperature, and then stretched and shaped at a speed of 800 m / min, and finally divided and wound to obtain spun fibers; the spun fibers are heat treated at 320°C for 15 hours to obtain finished fibers.
[0056] Example 4
[0057] According to the 1# ratio, monomers p-hydroxybenzoic acid, 1,1'-bi-2-naphthol, terephthalic acid, acylating agent acetic anhydride accounting for 1.6 times the total molar number of hydroxyl groups of the three monomers, and catalyst 2-(4-methylpiperazine)-3-aminopyridine accounting for 500ppm of the total weight of the three monomers are put into a Hastelloy kettle and kept at 150°C for 1 hour, then the temperature is raised to 330°C and kept for 1 hour, and then 1.0MPa of inert gas is filled into the Hastelloy kettle, and the reaction product material is discharged through a discharge valve with a diameter of 2mm and 10 holes, crushed, passed through a 30-mesh sieve, and dried at 130°C for 1 hour to obtain the prepolymer; in an inert gas atmosphere, the prepolymer is subjected to solid phase polycondensation reaction at 330°C for 12 hours to obtain a polycondensate; the obtained polycondensate is mixed and extruded with 2,5-bipyridinecarboxylic acid at 330°C in a screw extruder with a rotation speed of 300r / min at 300°C to obtain a liquid crystal polymer.
[0058] The liquid crystal polymer is heated to 330°C and then extruded, supplied to a spinning assembly, through which fiber filaments are ejected, the fiber filaments are kept at 300°C for 5 minutes, then air-cooled to room temperature, and then stretched and shaped at a speed of 900 m / min, and finally divided and wound to obtain spun fibers; the spun fibers are heat treated at 330°C for 12 hours to obtain finished fibers.
[0059] Comparative Example 1
[0060] The only difference from Embodiment 1 is that the monomer 2,5-dipyridinecarboxylic acid is added together with hydroxybenzoic acid, 1,1'-bi-2-naphthol, terephthalic acid, acylating agent acetic anhydride and catalyst 2-(4-methylpiperazine)-3-aminopyridine into a Hastelloy kettle for polymerization reaction.
[0061] Comparative Example 2
[0062] The only difference from Example 1 is that 2,6-naphthalenediol is used in an equal molar fraction to replace 1,1'-bi-2-naphthol.
[0063] Comparative Example 3
[0064] The only difference from Example 1 is that terephthalic acid is used in an equal molar fraction to replace 2,5-bipyridinecarboxylic acid.
[0065] Comparative Example 4
[0066] The only difference from Example 1 is that an equal amount of potassium acetate is used to replace 2-(4-methylpiperazine)-3-aminopyridine as a catalyst to participate in the polymerization reaction.
[0067] The relevant performance testing method of the liquid crystal polymer fiber of the present invention is as follows:
[0068] (1) Tensile strength: The tensile strength test was carried out according to ISO 527-2 standard;
[0069] (2) Friction resistance test: According to GB / T9996 standard, the friction test was carried out using a raw silk cohesion tester. The tensile strength was measured after 5000 frictions, and the degree of fuzzing on the fiber surface was observed with the naked eye.
[0070] (3) Friction coefficient: Take a stainless steel rod with a diameter of 50 mm and a chrome-plated surface. Fix the filament shaft and wrap the fiber around the stainless steel rod for half a circle (the fiber wrap angle is 180°). A heavy weight T1 is fixed at one end of the fiber. A digital tensile gauge is used to measure the tension T2 at the other end of the fiber. The fiber friction coefficient μμ = (1 / π) × ln(T2 / T1).
[0071] The results of Examples 1-4 and Comparative Examples 1-4 measured using the above performance testing method are shown in Table (2).
[0072] Table (2): Performance test results of Examples 1-4 and Comparative Examples 1-4
[0073]
[0074] It can be seen from the above examples that the liquid crystal polymer fiber obtained by adopting the technical solution of the present invention not only has good wear resistance, but also has a suitable friction coefficient, which fully meets the application requirements of transmission belts.
[0075] The above-mentioned implementation mode is only a preferred technical solution of the present invention. Any other changes, modifications, substitutions, combinations and simplifications made without departing from the spirit and working principle of the present invention shall be equivalent replacement methods and shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a liquid crystal polymer, characterized in that: The preparation method comprises the following steps: A1: mixing monomers p-hydroxybenzoic acid, 1,1'-bi-2-naphthol, terephthalic acid with an acylating agent and a catalyst to obtain a reaction mixture; wherein, by mole, the mole fractions of the three monomers are as follows: 100 parts of p-hydroxybenzoic acid, 5-15 parts of 1,1'-bi-2-naphthol, and 3-10 parts of terephthalic acid; A2: subjecting the reaction mixture to a prepolymerization reaction to obtain a prepolymer; A3: Under an inert gas atmosphere, subjecting the prepolymer to a solid phase polycondensation reaction to obtain a polycondensate; A4: The obtained polycondensate is mixed with 2-5 mole parts of 2,5-bipyridinecarboxylic acid in a screw extruder and extruded to obtain a liquid crystal polymer.
2. The method for preparing a liquid crystal polymer according to claim 1, wherein: The sum of the molar fractions of terephthalic acid and 2,5-bipyridinecarboxylic acid is equal to the molar fraction of 1,1'-bi-2-naphthol.
3. The method for preparing a liquid crystal polymer according to claim 1, wherein: The catalyst is 2-(4-methylpiperazine)-3-aminopyridine, and the added amount is 400-500ppm of the total weight of the three monomers of p-hydroxybenzoic acid, 1,1'-bi-2-naphthol and terephthalic acid.
4. The method for preparing a liquid crystal polymer according to claim 1, wherein: In step A4, the extrusion temperature of the screw extruder is 300-330°C.
5. A liquid crystal polymer, characterized in that: The liquid crystal polymer is prepared by the preparation method of the liquid crystal polymer according to any one of claims 1 to 4.
6. A method for preparing a liquid crystal polymer fiber, characterized in that: The preparation method comprises the following steps: a1: heating and extruding the liquid crystal polymer as claimed in claim 5, supplying the polymer to a spinning assembly, ejecting fiber filaments through the spinning assembly, and subjecting the fiber filaments to heat preservation, air cooling, drawing and shaping, and filament separation and winding to obtain nascent fibers; a2: heat-treating the spun fibers to obtain finished fibers.
7. The method for preparing liquid crystal polymer fiber according to claim 6, characterized in that: The insulation temperature in the step a1 is 280-300° C., and the speed of the drawing and shaping is 800-900 m / min.
8. The method for preparing liquid crystal polymer fiber according to claim 6, characterized in that: The heat treatment temperature in step a2 is 280-330° C. and the time is 12-24 hours.
9. A liquid crystal polymer fiber, characterized in that: The liquid crystal polymer fiber is prepared by the preparation method of the liquid crystal polymer fiber according to any one of claims 6 to 8.