High-wear-resistance, anti-dazzle and antireflection optical film and preparation method thereof
By using fluorine-containing acrylate modified cage polysilsesquioxane and other components in the optical film, a high wear-resistant, anti-glare anti-reflective film is formed, which solves the problem of high haze and poor friction resistance in the prior art. Problem, low reflectivity and high wear resistance are achieved, and the anti-glare effect of the optical film is significantly improved.
Patent Information
- Application Number
- CN202411032934.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-12
AI Technical Summary
The existing anti-glare anti-reflective film has too high haze and poor friction resistance, which cannot effectively reduce the reflection of strong light inside the flat panel display, resulting in visual fatigue and surface damage.
Using a high wear-resistant, anti-glare anti-reflective optical film including base film, anti-glare coating and anti-reflective coating, the anti-reflective coating is used to modify the cage polysilsesquioxane in the anti-reflective coating, and is cured by UV. Components such as resin, modified hollow silica particles and photoinitiator have excellent scratch resistance and anti-reflection effect.
It achieves low reflectivity, low haze and high wear resistance, and can be scratched after 1kg/2600 dust-free cloth friction, which significantly improves the anti-glare and wear resistance of the optical film.
Smart Images

Figure CN118930932A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of optical film materials, and in particular to a highly wear-resistant, anti-glare and anti-reflection optical film and a preparation method thereof. Background Art
[0002] In recent years, with the rapid development of the flat panel display industry, the development of many key upstream basic materials of flat panel displays, such as thin film materials, has been driven.
[0003] When a flat panel display is working, strong light is generated inside and reflected to the outer surface. When the human eye is under the display for a long time, it is very easy to cause visual fatigue and damage vision. Therefore, it is necessary to perform anti-glare treatment on the surface of the display to reduce the impact of strong light inside the display or reduce the intensity of reflected light to improve transmittance.
[0004] In addition, during the use of flat panel displays, fingerprints will be left due to frequent human contact, and excessive force will cause surface damage when cleaning the display surface. Therefore, it is necessary to give the surface of the optical film for flat panel displays high friction resistance and anti-fingerprint functions.
[0005] However, the main company that can produce such anti-glare and anti-reflection films on the market is Daicel Corporation of Japan. Daicel Corporation of Japan prepares anti-glare and anti-reflection films in patent publication number CN 111433641 A, but its haze is too high, friction resistance, and anti-reflection performance are poor. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a highly wear-resistant, anti-glare and anti-reflection optical film and a preparation method thereof in view of the above-mentioned deficiencies in the prior art. The optical film of the present invention has both excellent anti-reflection effect and provides the anti-reflection coating surface with scratch resistance and excellent anti-glare effect.
[0007] To achieve the above-mentioned purpose, the technical solution adopted by the present invention is as follows: In a first aspect of the present invention, a highly wear-resistant, anti-glare and anti-reflection optical film is provided, comprising a base film, an anti-glare coating formed on the base film, and an anti-reflection coating formed on the anti-glare coating:
[0008] The anti-reflection coating is obtained by coating an anti-reflection coating liquid and then curing the anti-reflection coating liquid, wherein the anti-reflection coating liquid comprises the following raw material components in parts by weight: 6-24 parts of UV curable resin, 0.3-1.2 parts of active diluent monomer, 2.5-10 parts of modified hollow silica particle dispersion with a solid content of 10-40%, 0.35-1.4 parts of a first photoinitiator, 0.5-1.5 parts of fluorine-containing acrylate modified cage-type polysilsesquioxane, 1-4 parts of AF additive, and 140-560 parts of a first organic solvent.
[0009] Preferably, the fluorinated acrylate modified cage-type polysilsesquioxane is prepared by the following method:
[0010] 1-1) under nitrogen protection and light-proof conditions, isophorone diisocyanate, acrylate and a catalyst are mixed, heated and stirred to obtain isocyanate-modified acrylate;
[0011] 1-2) mixing isocyanate-modified acrylate, hydroxyl fluorinated acrylate and catalyst, heating for reaction, adding pentaerythritol triacrylate for dilution after the reaction, and removing the solvent in the product by vacuum distillation to obtain double-bond terminated fluorinated acrylate: FPU;
[0012] 1-3) (3-mercaptopropyl)trimethoxysilane is dissolved in methanol, hydrochloric acid is added dropwise while stirring, and the mixture is condensed and refluxed under heating. After the reaction is completed, the mixture is cooled and separated, and the upper clear liquid is discarded. A solvent is added to the remaining product to dissolve the mixture, and the resulting mixture is added to a methanol solvent for precipitation. After standing, the upper clear liquid is discarded, and the lower layer is the product, which is dried in vacuo to obtain the product octamercapto cage-type polysilsesquioxane: POSS-SH;
[0013] 1-4) Grafting FPU onto the thiol group of POSS-SH by click reaction: POSS-SH is dissolved in a solvent, and FPU and 2,2-dihydroxymethylpropionic acid photoinitiator are added, and the mixture is stirred until it is completely dissolved, irradiated with ultraviolet light, and then the solvent is removed by rotary evaporation. After vacuum drying, the product fluorinated acrylate modified cage-type polysilsesquioxane: FPU-POSS is obtained.
[0014] Preferably, the fluorinated acrylate modified cage-type polysilsesquioxane is prepared by the following method:
[0015] 1-1) Under nitrogen protection and light-proof conditions, 100-120 g of isophorone diisocyanate and 0.04-0.06 g of a catalyst are added to a reaction vessel, the temperature is raised to 35-45° C., and then 55-70 g of acrylate is added dropwise to the reaction vessel, and the reaction is stirred at 45-50° C. The reaction endpoint is monitored by measuring the NCO value, and the reaction is terminated when the NCO value is 48-55%. After the reaction is completed, isocyanate-modified acrylate is obtained;
[0016] 1-2) the isocyanate-modified acrylate and the hydroxyl fluorinated acrylate prepared in step 1-1) are mixed in a molar ratio of 1.1:1, 0.0025-0.01 g of dibutyltin dilaurate as a catalyst is added dropwise while stirring, and the reaction is stirred at 40-60° C. for 1-2 h, and the reaction endpoint is monitored by measuring the NCO value. When the NCO value is less than 0.5%, the reaction is terminated. After the reaction is completed, pentaerythritol triacrylate is added for dilution, and the solvent in the product is removed by vacuum distillation to obtain a double-bond terminated fluorinated acrylate: FPU;
[0017] 1-3) 9.8 g (3-mercaptopropyl) trimethoxysilane was dissolved in methanol, and 30 mL of concentrated hydrochloric acid with a mass concentration of 36-38% was added dropwise while stirring, and the mixture was condensed and refluxed at 80-100° C. for 12-36 h. After the reaction was completed, the mixture was cooled and layered, and the supernatant was discarded. Dichloromethane was added to the remaining product to dissolve the mixture, and the mixture was added to methanol solvent for precipitation. After standing for 3-5 h, the supernatant was discarded, and the lower layer was the product, which was vacuum dried at 50-70° C. for 4-16 h to obtain the product octamercapto cage-type polysilsesquioxane: POSS-SH;
[0018] 1-4) Grafting FPU on the thiol group of POSS-SH by click reaction: 1-2g POSS-SH is added to 60-250mL tetrahydrofuran solvent, and 10-20g FPU and 0.25-1g 2,2-dihydroxymethylpropionic acid (DMPA) photoinitiator are added, and magnetic stirring is performed until the mixture is completely dissolved, and ultraviolet light is irradiated for 15-60min, and then the tetrahydrofuran solvent is removed by rotary evaporation at 40-60°C, and vacuum drying is performed at 50-70°C for 4-16h to obtain the product fluorinated acrylate modified cage-type polysilsesquioxane: FPU-POSS.
[0019] Preferably, the UV curable resin is one or more of fluorocarbon modified polyurethane acrylate, fluorosilicone modified polyurethane acrylate, fluorocarbon modified polyester acrylate, and fluorosilicone modified polyester acrylate;
[0020] The active monomer is one or more of pentaerythritol triacrylate (PETA), pentaerythritol tetraacrylate (PETTA), dipentaerythritol pentaacrylate (DPPA), and dipentaerythritol hexaacrylate (DPHA);
[0021] The first photoinitiator is one or more of 184, 1173, TPO, KIP 150, 160, and Esacure ONE;
[0022] AF additives are fluorinated acrylate compounds;
[0023] The first organic solvent is one or more of propylene glycol methyl ether (PM), methyl isobutyl ketone (MIBK), ethyl acetate (EAC), and butanone (MEK).
[0024] Preferably, the anti-reflective coating is prepared by the following method: UV curable resin, active diluent monomer, modified hollow silica particles, a first photoinitiator, fluorinated acrylate modified cage polysilsesquioxane, AF additive, and a first organic solvent are uniformly mixed to obtain an anti-reflective coating.
[0025] Preferably, the anti-glare coating is obtained by coating an anti-glare coating liquid and then curing it, and the anti-glare coating liquid includes the following raw material components in parts by weight: 1.35-5.4 parts of anti-glare micron particles, 0.4-1.6 parts of dispersant, 35-150 parts of a second organic solvent, 17.5-70 parts of a high hardness and high wear-resistant resin, 4-16 parts of a dual-curing resin, 1-4 parts of a second photoinitiator, and 0.1-0.4 parts of a leveling agent.
[0026] Preferably, the anti-glare coating is prepared by the following method:
[0027] 2-1) mixing the anti-glare micron particles, the dispersant and the second organic solvent, and stirring at 800-3200 r / min for 2-8 hours to obtain an anti-glare base coating slurry;
[0028] 2-2) mixing a high-hardness and high-wear-resistant resin, a dual-curing resin, a second photoinitiator, and a second organic solvent, and stirring at 450-1800 r / min for 30-120 min to obtain an anti-glare base coating clear liquid;
[0029] 2-3) The anti-glare base coating slurry and the anti-glare base coating clear liquid are mixed, and then a leveling agent is added. After stirring evenly, the mixture is allowed to stand for defoaming for 15-60 minutes to obtain the anti-glare coating liquid.
[0030] Preferably, the anti-glare micron particles are one or both of modified silica particles and modified PMMA particles.
[0031] The dispersant is one or more of modified polyacrylate, acrylic block copolymer, and modified polyurethane;
[0032] The high-hardness and high-wear-resistant resin is polyurethane acrylate, with a functionality of 6-9 and a viscosity of 800-5000 mPa·s;
[0033] The dual-cure resin is polyurethane-modified acrylic epoxy monoester, with a functionality of 6-9 and a viscosity of 500-5000 mPa·s;
[0034] The second photoinitiator is one or more of 184, 1173, TPO, KIP 150, 160, and Esacure ONE;
[0035] The second organic solvent is one or more of propylene glycol methyl ether (PM), methyl isobutyl ketone (MIBK), ethyl acetate (EAC), and butanone (MEK).
[0036] Preferably, the base film is a PET film, a PC film or a TAC film, and has a thickness of 40-100 μm.
[0037] The second aspect of the present invention provides a method for preparing the highly wear-resistant, anti-glare and anti-reflection optical film as described above, comprising the following steps:
[0038] S1. Apply the anti-glare coating evenly on the surface of the base film, bake at 80-100℃ for 1-4min, and then UV cure. Control the UV curing energy to 300-500mJ / cm 2 , forming an anti-glare coating;
[0039] S2. Evenly apply the anti-reflection coating on the anti-glare coating, bake at 80-100℃ for 1-4min, and then UV cure. Control the UV curing energy to 600-800mJ / cm 2 , forming an anti-reflection coating to obtain the highly wear-resistant, anti-glare anti-reflection optical film.
[0040] The beneficial effects of the present invention are:
[0041] The invention provides a highly wear-resistant, anti-glare and anti-reflection optical film. The invention adopts anti-glare particles to reduce the reflected light on the surface of the coating so as to achieve the anti-glare effect. Fluorine-containing acrylate-modified cage-type polysilsesquioxane is applied to the anti-reflection coating. Due to the regular spatial structure of the cage-type polysilsesquioxane (POSS), the group R connected to the Si atom is designed and grafted with unsaturated double bonds. Compared with traditional blends, the interface stability is better, the film has good compatibility with UV curing resins, can participate in photocuring reactions, and improves the conversion rate of photocuring double bonds. The prepared anti-reflection coating has excellent wear resistance and optical properties.
[0042] In some preferred embodiments of the present invention, the prepared highly wear-resistant, anti-glare and anti-reflection film has a light reflectivity of less than 2.5%, a haze of 18-20%, and a wear resistance of 1kg / 2600 times of dust-free cloth friction without scratches. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 It is a schematic structural diagram of the highly wear-resistant, anti-glare and anti-reflection optical film of the present invention;
[0044] Figure 2 The invention discloses a preparation route of the fluorinated acrylate modified cage-type polysilsesquioxane.
[0045] Description of reference numerals:
[0046] 1-base film; 2-anti-glare coating; 3-anti-reflection coating; 4-anti-glare micron particles; 5-modified hollow silica particles. DETAILED DESCRIPTION
[0047] The present invention is further described in detail below in conjunction with embodiments so that those skilled in the art can implement the invention with reference to the description.
[0048] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.
[0049] The test methods used in the following examples are conventional methods unless otherwise specified. The materials and reagents used in the following examples are all commercially available unless otherwise specified. In the following examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.
[0050] The present invention provides a highly wear-resistant, anti-glare and anti-reflection optical film, comprising a base film, an anti-glare coating formed on the base film, and an anti-reflection coating formed on the anti-glare coating:
[0051] The anti-reflection coating is obtained by coating an anti-reflection coating liquid and then curing the anti-reflection coating liquid. The anti-reflection coating liquid includes the following raw material components by weight: 6-24 parts of UV curable resin, 0.3-1.2 parts of active diluent monomer, 2.5-10 parts of modified hollow silica particle dispersion with a solid content of 10-40%, 0.35-1.4 parts of a first photoinitiator, 0.5-1.5 parts of fluorine-containing acrylate modified cage-type polysilsesquioxane, 1-4 parts of AF additive, and 140-560 parts of a first organic solvent.
[0052] In a preferred embodiment, the fluorinated acrylate modified cage-type polysilsesquioxane is prepared by the following method:
[0053] 1-1) under nitrogen protection and light-proof conditions, isophorone diisocyanate, acrylate and a catalyst are mixed, heated and stirred to obtain isocyanate-modified acrylate;
[0054] 1-2) mixing isocyanate-modified acrylate, hydroxyl fluorinated acrylate and catalyst, heating for reaction, adding pentaerythritol triacrylate for dilution after the reaction, and removing the solvent in the product by vacuum distillation to obtain double-bond terminated fluorinated acrylate: FPU;
[0055] 1-3) (3-mercaptopropyl)trimethoxysilane is dissolved in methanol, hydrochloric acid is added dropwise while stirring, and the mixture is condensed and refluxed under heating. After the reaction is completed, the mixture is cooled and separated, and the upper clear liquid is discarded. A solvent is added to the remaining product to dissolve the mixture, and the resulting mixture is added to a methanol solvent for precipitation. After standing, the upper clear liquid is discarded, and the lower layer is the product, which is dried in vacuo to obtain the product octamercapto cage-type polysilsesquioxane: POSS-SH;
[0056] 1-4) Grafting FPU onto the thiol group of POSS-SH by click reaction: POSS-SH is dissolved in a solvent, and FPU and 2,2-dihydroxymethylpropionic acid photoinitiator are added, and the mixture is stirred until it is completely dissolved, irradiated with ultraviolet light, and then the solvent is removed by rotary evaporation. After vacuum drying, the product fluorinated acrylate modified cage-type polysilsesquioxane: FPU-POSS is obtained.
[0057] In a preferred embodiment, the fluorinated acrylate modified cage-type polysilsesquioxane is prepared by the following method:
[0058] 1-1) Under nitrogen protection and light-proof conditions, 100-120 g of isophorone diisocyanate and 0.04-0.06 g of a catalyst are added to a reaction vessel, the temperature is raised to 35-45° C., and then 55-70 g of acrylate is added dropwise to the reaction vessel, and the reaction is stirred at 45-50° C. The reaction endpoint is monitored by measuring the NCO value, and the reaction is terminated when the NCO value is 48-55%. After the reaction is completed, isocyanate-modified acrylate is obtained;
[0059] 1-2) the isocyanate-modified acrylate and the hydroxyl fluorinated acrylate prepared in step 1-1) are mixed in a molar ratio of 1.1:1, 0.0025-0.01 g of dibutyltin dilaurate as a catalyst is added dropwise while stirring, and the reaction is stirred at 40-60° C. for 1-2 h, and the reaction endpoint is monitored by measuring the NCO value. When the NCO value is less than 0.5%, the reaction is terminated. After the reaction is completed, pentaerythritol triacrylate is added for dilution, and the solvent in the product is removed by vacuum distillation to obtain a double-bond terminated fluorinated acrylate: FPU;
[0060] 1-3) 9.8 g (3-mercaptopropyl) trimethoxysilane was dissolved in methanol, and 30 mL of concentrated hydrochloric acid with a mass concentration of 36-38% was added dropwise while stirring, and the mixture was condensed and refluxed at 80-100° C. for 12-36 h. After the reaction was completed, the mixture was cooled and layered, and the supernatant was discarded. Dichloromethane was added to the remaining product to dissolve the mixture, and the mixture was added to methanol solvent for precipitation. After standing for 3-5 h, the supernatant was discarded, and the lower layer was the product, which was vacuum dried at 50-70° C. for 4-16 h to obtain the product octamercapto cage-type polysilsesquioxane: POSS-SH;
[0061] 1-4) Grafting FPU on the thiol group of POSS-SH by click reaction: 1-2g POSS-SH is added to 60-250mL tetrahydrofuran solvent, and 10-20g FPU and 0.25-1g 2,2-dihydroxymethylpropionic acid (DMPA) photoinitiator are added, and magnetic stirring is performed until the mixture is completely dissolved, and ultraviolet light is irradiated for 15-60min, and then the tetrahydrofuran solvent is removed by rotary evaporation at 40-60°C, and vacuum drying is performed at 50-70°C for 4-16h to obtain the product fluorinated acrylate modified cage-type polysilsesquioxane: FPU-POSS.
[0062] In a preferred embodiment, the UV curable resin is one or more of fluorocarbon modified polyurethane acrylate, fluorosilicone modified polyurethane acrylate, fluorocarbon modified polyester acrylate, and fluorosilicone modified polyester acrylate; more preferably, it is an organic fluorine modified high-functional aliphatic polyurethane acrylate with a functionality of 10-15 and a viscosity of 20000-60000 mPa·s.
[0063] In a preferred embodiment, the active monomer is one or more of pentaerythritol triacrylate (PETA), pentaerythritol tetraacrylate (PETTA), dipentaerythritol pentaacrylate (DPPA), and dipentaerythritol hexaacrylate (DPHA).
[0064] In a preferred embodiment, the first photoinitiator is a free radical photoinitiator, including small molecule and macromolecular photoinitiators, for example, one or more of 184, 1173, TPO, KIP 150, 160, and Esacure ONE.
[0065] In a preferred embodiment, the AF auxiliary agent is a fluorine-containing acrylate compound.
[0066] In a preferred embodiment, the first organic solvent is one or more of propylene glycol methyl ether (PM), methyl isobutyl ketone (MIBK), ethyl acetate (EAC), and butanone (MEK).
[0067] In a preferred embodiment, the modified hollow silica nanoparticles have a particle size of 20-50 nm, a wall thickness of 10 nm, and a porosity of 45-55%.
[0068] In a preferred embodiment, the anti-reflective coating is prepared by the following method: UV curable resin, active diluent monomer, modified hollow silica particles, a first photoinitiator, fluorinated acrylate modified cage polysilsesquioxane, AF additive, and a first organic solvent are uniformly mixed to obtain an anti-reflective coating.
[0069] In the present invention, the anti-glare coating is obtained by coating an anti-glare coating liquid and then curing it. The anti-glare coating liquid includes the following raw material components in parts by weight: 1.35-5.4 parts of anti-glare micron particles, 0.4-1.6 parts of a dispersant, 35-150 parts of a second organic solvent, 17.5-70 parts of a high-hardness and high-wear-resistant resin, 4-16 parts of a dual-curing resin, 1-4 parts of a second photoinitiator, and 0.1-0.4 parts of a leveling agent.
[0070] In a preferred embodiment, the anti-glare coating is prepared by the following method:
[0071] 2-1) mixing the anti-glare micron particles, the dispersant and the second organic solvent, and stirring at 800-3200 r / min for 2-8 hours to obtain an anti-glare base coating slurry;
[0072] 2-2) mixing a high-hardness and high-wear-resistant resin, a dual-curing resin, a second photoinitiator, and a second organic solvent, and stirring at 450-1800 r / min for 30-120 min to obtain an anti-glare base coating clear liquid;
[0073] 2-3) The anti-glare base coating slurry and the anti-glare base coating clear liquid are mixed, and then a leveling agent is added. After stirring evenly, the mixture is allowed to stand for defoaming for 15-60 minutes to obtain an anti-glare coating liquid.
[0074] In a preferred embodiment, the anti-glare micron particles are organic or inorganic micron particles, for example, one or both of modified silica particles and modified PMMA particles.
[0075] In a preferred embodiment, the dispersant is one or more of modified polyacrylate, acrylic block copolymer, and modified polyurethane.
[0076] In a preferred embodiment, the high hardness and high wear-resistant resin is polyurethane acrylate with a functionality of 6-9 and a viscosity of 800-5000 mPa·s.
[0077] In a preferred embodiment, the dual-cure resin is polyurethane-modified epoxy acrylate monoester with a functionality of 6-9 and a viscosity of 500-5000 mPa·s.
[0078] In a preferred embodiment, the second photoinitiator is a free radical photoinitiator, including small molecule and macromolecular photoinitiators, for example, one or more of 184, 1173, TPO, KIP 150, 160, and Esacure ONE.
[0079] In a preferred embodiment, the second organic solvent is one or more of propylene glycol methyl ether (PM), methyl isobutyl ketone (MIBK), ethyl acetate (EAC), and butanone (MEK).
[0080] In a preferred embodiment, the base film is an optical-grade PET film, PC film or TAC film with a thickness of 40-100 μm, such as 40 μm, 50 μm, 60 μm, 65 μm, 75 μm, 80 μm, 100 μm, etc.
[0081] The present invention also provides a method for preparing the above highly wear-resistant, anti-glare and anti-reflection optical film, comprising the following steps:
[0082] S1. Apply the anti-glare coating evenly on the surface of the base film, bake at 80-100℃ for 1-4min, and then UV cure. Control the UV curing energy to 300-500mJ / cm 2 , forming an anti-glare coating with low water contact, high hardness and high wear resistance;
[0083] S2. Evenly apply the anti-reflection coating on the anti-glare coating, bake at 80-100℃ for 1-4min, and then UV cure. Control the UV curing energy to 600-800mJ / cm 2 , forming an anti-reflection coating to obtain a highly wear-resistant, anti-glare anti-reflection optical film.
[0084] The high wear-resistant anti-glare anti-reflection film of the present invention has a light reflectivity of less than 2.5%, a haze of 18-20%, and a wear resistance of 1kg / 2600 times without scratches after being rubbed with a dust-free cloth.
[0085] Reference Figure 1 , is a schematic diagram of the structure of the highly wear-resistant, anti-glare and anti-reflection optical film of the present invention, which comprises a base film 1, an anti-glare coating 2 and an anti-reflection coating 3, wherein the anti-glare coating 2 contains anti-glare micron particles 4, and the anti-reflection coating 3 contains modified hollow silica particles 5.
[0086] The present invention uses a transparent optical film as a substrate, and forms an anti-glare coating on the transparent optical grade base film and an anti-reflection coating on the anti-glare coating. The anti-glare coating contains a high wear-resistant resin, a dual-cured resin, micro-nano anti-glare particles, a photoinitiator, a solvent, and other additives. The anti-glare coating has a haze of 18-20% due to the micro-nano anti-glare particles that coarsen the surface of the coating, weaken the specular reflection of the coating surface, and achieve an anti-glare effect; the anti-reflection coating contains UV curing resin, high-functionality polyurethane acrylate, active monomer, modified hollow silica, fluorine-containing acrylate modified cage-type polysilsesquioxane, AF additive, photoinitiator, and solvent. In the anti-reflection coating, the cage-type polysilsesquioxane is modified by fluorine-containing acrylate, so that the surface of the cage-type polysilsesquioxane has both fluorine-containing acrylate to reduce the dynamic friction coefficient of the coating and chemical bonds that can react with the anti-reflection coating, so that the modified cage-type polysilsesquioxane can be more firmly connected to the main body of the anti-reflection coating to improve the wear resistance of the coating.
[0087] The above is the overall concept of the present invention, and detailed embodiments and comparative examples are provided below on the basis of the overall concept of the present invention to further illustrate the present invention.
[0088] The fluorinated acrylate modified cage-type polysilsesquioxane involved in the following examples and comparative examples is prepared by the following method:
[0089] 1-1) Under nitrogen protection and light-proof conditions, 110 g of isophorone diisocyanate and 0.05 g of a catalyst were added to a reaction vessel, the temperature was raised to 40° C., and then 60 g of acrylate was added dropwise to the reaction vessel. The reaction was stirred at 45° C., and the reaction endpoint was monitored by measuring the NCO value. The reaction was terminated when the NCO value was 50%. After the reaction was completed, isocyanate-modified acrylate was obtained;
[0090] 1-2) the isocyanate-modified acrylate and the hydroxyl fluorinated acrylate prepared in step 1-1) are mixed in a molar ratio of 1.1:1, 0.005 g of a catalyst dibutyltin dilaurate is added dropwise while stirring, and the reaction is stirred at 50° C. for 1-2 hours, and the reaction end point is monitored by measuring the NCO value. When the NCO value is less than 0.5%, the reaction is terminated. After the reaction is completed, pentaerythritol triacrylate is added for dilution, and the solvent in the product is removed by vacuum distillation to obtain a double-bond terminated fluorinated acrylate: FPU;
[0091] 1-3) 9.8 g (3-mercaptopropyl) trimethoxysilane was dissolved in methanol, and 30 mL of concentrated hydrochloric acid with a mass concentration of 36% was added dropwise while stirring, and condensed and refluxed at 90° C. for 24 h. After the reaction was completed, the mixture was cooled and layered, and the supernatant was poured out. Dichloromethane solvent was added to the remaining product to dissolve it, and the resulting mixture was added to methanol solvent for precipitation. After standing for 4 h, the supernatant was poured out, and the lower layer was the product, which was vacuum dried at 60° C. for 8 h to obtain the product octamercapto cage-type polysilsesquioxane: POSS-SH;
[0092] 1-4) Grafting FPU on the thiol group of POSS-SH by click reaction: 1.5 g POSS-SH was added to 125 mL tetrahydrofuran solvent, and 15 g FPU and 0.5 g 2,2-dihydroxymethylpropionic acid (DMPA) photoinitiator were added, and magnetic stirring was performed until the mixture was completely dissolved, and ultraviolet light (LED 365 nm) was irradiated for 30 min, and then the product was poured into a round-bottom flask, and the tetrahydrofuran solvent was removed by rotary evaporation at 50°C, and vacuum dried at 60°C for 4-16 h to obtain the product fluorinated acrylate modified cage-type polysilsesquioxane: FPU-POSS.
[0093] The preparation route is as follows Figure 2 shown.
[0094] Example 1
[0095] A highly wear-resistant, anti-glare and anti-reflection optical film, the preparation method of which comprises the following steps:
[0096] S1. Use a 30# wire rod to evenly coat the anti-glare coating liquid on the surface of the base film (optical grade transparent PET film, thickness of 75μm), bake at 80℃ for 2min, and then UV cure. Control the UV curing energy to 300mJ / cm 2 , forming an anti-glare coating with low water contact, high hardness and high wear resistance;
[0097] S2. Use a 5# wire rod to evenly coat the anti-reflection coating on the anti-glare coating, bake at 80℃ for 2 minutes, and then UV cure. Control the UV curing energy to 800mJ / cm 2 , under nitrogen protection, it is cured to form an anti-reflection coating to obtain a highly wear-resistant, anti-glare and anti-reflection optical film.
[0098] Wherein, the anti-glare coating solution is prepared by the following method:
[0099] 1) 20 parts by weight of solvent PM and dispersant (BASF, PX 4310) 0.8 weight parts were stirred for 10 min to mix evenly, and then 2.7 weight parts of anti-glare micron particles (Evonik Chemical, OK520) were added and stirred at high speed (1600r / min) for 4h, and then allowed to stand and defoam for 1h to obtain an anti-glare base coating slurry for standby use;
[0100] 2) 35 parts by weight of high-hardness and high-wear-resistant resin (Nanjing Sanan, SN6300), 8 parts by weight of dual-cure resin (Taiwan, China, Ouli, DTP9005), 2 parts by weight of photoinitiator 184 (BASF), and 40 / 15 parts by weight of organic solvent mixture (PM / MEK) were mixed and stirred for 1 hour at a speed of 900 r / min, and allowed to stand to obtain an anti-glare base coating clear liquid for standby use;
[0101] 3) The anti-glare base coating slurry and the anti-glare base coating clear liquid were mixed, and 0.2 parts by weight of a leveling agent (BYK Chemical, BYK310) was added. After stirring evenly, the mixture was allowed to stand for defoaming for 30 minutes to obtain an anti-glare coating liquid for use.
[0102] Wherein, the anti-reflection coating liquid is prepared by the following method:
[0103] 12 parts by weight of UV curing resin (Guangzhou Songda, SD 1338B), 0.6 parts by weight of DPHA (Sartomer), 5 parts by weight of modified hollow silica dispersion (JGC Catalysts & Chemicals, THRULYA4320, solid content 20%), 0.7 parts by weight of photoinitiator KIP 150, 1 part by weight of fluorinated acrylate modified cage-type polysilsesquioxane, 2 parts by weight of AF additive (Zhongfu Technology, Fluere UV-370), and an organic solvent (a mixed solvent of 130 parts by weight of MEK and 150 parts by weight of MIBK) were mixed, stirred at 800 rpm for 1.5 hours, allowed to stand, and defoamed for 12 hours to obtain an anti-reflective optical coating for standby use, with a refractive index of 1.45.
[0104] Example 2
[0105] A highly wear-resistant, anti-glare and anti-reflection optical film, the preparation method of which comprises the following steps:
[0106] S1. Use a 25# wire rod to evenly coat the anti-glare coating liquid on the surface of the base film (optical grade transparent PET film, thickness of 75μm), bake at 80℃ for 2min, and then UV cure. Control the UV curing energy to 300mJ / cm 2 , forming an anti-glare coating with low water contact, high hardness and high wear resistance;
[0107] S2. Use a 5# wire rod to evenly coat the anti-reflection coating on the anti-glare coating, bake at 80℃ for 2 minutes, and then UV cure. Control the UV curing energy to 800mJ / cm 2 , under nitrogen protection, it is cured to form an anti-reflection coating to obtain a highly wear-resistant, anti-glare and anti-reflection optical film.
[0108] The anti-glare coating liquid is the same as that in Example 1.
[0109] Wherein, the anti-reflection coating liquid is prepared by the following method:
[0110] 11 parts by weight of UV curing resin (Guangzhou Songda, SD 1338B), 0.6 parts by weight of DPHA (Sartomer), 5 parts by weight of modified hollow silica dispersion (JGC Catalysts & Chemicals, THRULYA4320, solid content 20%), 0.7 parts by weight of photoinitiator KIP 150, 0.7 parts by weight of fluorinated acrylate modified cage-type polysilsesquioxane, 2 parts by weight of AF additive (China Fluoro Technology, Fluere UV-370), and an organic solvent (a mixed solvent of 100 parts by weight of MEK and 180 parts by weight of MIBK) were mixed, stirred at 800 rpm for 1.5 hours, allowed to stand, and defoamed for 12 hours to obtain an anti-reflective optical coating for standby use, with a refractive index of 1.45.
[0111] Example 3
[0112] A highly wear-resistant, anti-glare and anti-reflection optical film, the preparation method of which comprises the following steps:
[0113] S1. Use a 25# wire rod to evenly coat the anti-glare coating liquid on the surface of the base film (optical grade transparent PET film, thickness of 75μm), bake at 80℃ for 2min, and then UV cure. Control the UV curing energy to 300mJ / cm 2 , forming an anti-glare coating with low water contact, high hardness and high wear resistance;
[0114] S2. Use a 5# wire rod to evenly coat the anti-reflection coating on the anti-glare coating, bake at 80℃ for 2 minutes, and then UV cure. Control the UV curing energy to 800mJ / cm 2 , under nitrogen protection, it is cured to form an anti-reflection coating to obtain a highly wear-resistant, anti-glare and anti-reflection optical film.
[0115] Wherein, the anti-glare coating solution is prepared by the following method:
[0116] 1) 20 parts by weight of solvent PM and dispersant (BASF, PX 4310) 0.8 weight parts were stirred for 10 min to mix evenly, and then 2.7 weight parts of anti-glare micron particles (Evonik Chemical, OK520) were added and stirred at high speed (1600r / min) for 4h, and then allowed to stand and defoam for 1h to obtain an anti-glare base coating slurry for standby use;
[0117] 2) 30 parts by weight of high-hardness and high-wear-resistant resin (Nanjing Sanan, SN6300), 10 parts by weight of dual-curing resin (Taiwan, China, Ouli, DTP9005), 2 parts by weight of photoinitiator 184 (BASF), and 40 / 15 parts by weight of organic solvent mixture (PM / MEK) were mixed and stirred for 1 hour at a speed of 900 r / min, and allowed to stand to obtain an anti-glare base coating clear liquid for standby use;
[0118] 3) The anti-glare base coating slurry and the anti-glare base coating clear liquid were mixed, and 0.2 parts by weight of a leveling agent (BYK Chemical, BYK310) was added. After stirring evenly, the mixture was allowed to stand for defoaming for 30 minutes to obtain an anti-glare coating liquid for use.
[0119] Wherein, the anti-reflection coating liquid is prepared by the following method:
[0120] 13 parts by weight of UV curing resin (Guangzhou Songda, SD 1338B), 0.65 parts by weight of DPHA (Sartomer), 5 parts by weight of modified hollow silica dispersion (JGC Catalysts & Chemicals, THRULYA4320, solid content 20%), 0.7 parts by weight of photoinitiator KIP 150, 1.2 parts by weight of fluorinated acrylate modified cage-type polysilsesquioxane, 2.6 parts by weight of AF additive (China Fluoro Technology, Fluere UV-370), and an organic solvent (a mixed solvent of 120 parts by weight of MEK and 200 parts by weight of MIBK) were mixed, stirred at 800 rpm for 1.5 hours, allowed to stand, and defoamed for 12 hours to obtain an anti-reflective optical coating for standby use, with a refractive index of 1.45.
[0121] Example 4
[0122] A highly wear-resistant, anti-glare and anti-reflection optical film, the preparation method of which comprises the following steps:
[0123] S1. Use a 25# wire rod to evenly coat the anti-glare coating liquid on the surface of the base film (optical grade transparent PET film, thickness of 75μm), bake at 80℃ for 2min, and then UV cure. Control the UV curing energy to 300mJ / cm 2 , forming an anti-glare coating with low water contact, high hardness and high wear resistance;
[0124] S2. Use a 5# wire rod to evenly coat the anti-reflection coating on the anti-glare coating, bake at 80℃ for 2 minutes, and then UV cure. Control the UV curing energy to 800mJ / cm 2 , under nitrogen protection, it is cured to form an anti-reflection coating to obtain a highly wear-resistant, anti-glare and anti-reflection optical film.
[0125] The anti-glare coating liquid is the same as that in Example 1.
[0126] Wherein, the anti-reflection coating liquid is prepared by the following method:
[0127] 13 parts by weight of UV curing resin (Guangzhou Songda, SD 1338B), 0.6 parts by weight of DPHA (Sartomer), 5.5 parts by weight of modified hollow silica dispersion (JGC Catalysts & Chemicals, THRULYA4320, solid content 20%), 0.7 parts by weight of photoinitiator KIP 150, 1 part by weight of fluorinated acrylate modified cage-type polysilsesquioxane, 2.6 parts by weight of AF additive (Zhongfu Technology, Fluere UV-370), and an organic solvent (a mixed solvent of 50 parts by weight of MEK and 300 parts by weight of MIBK) were mixed, stirred at 800 rpm for 1.5 hours, allowed to stand, and defoamed for 12 hours to obtain an anti-reflective optical coating for standby use, with a refractive index of 1.45.
[0128] Example 5
[0129] A highly wear-resistant, anti-glare and anti-reflection optical film, the preparation method of which comprises the following steps:
[0130] S1. Use a 25# wire rod to evenly coat the anti-glare coating liquid on the surface of the base film (optical grade transparent PET film, thickness of 75μm), bake at 80℃ for 2min, and then UV cure. Control the UV curing energy to 300mJ / cm 2 , forming an anti-glare coating with low water contact, high hardness and high wear resistance;
[0131] S2. Use a 5# wire rod to evenly coat the anti-reflection coating on the anti-glare coating, bake at 80℃ for 2 minutes, and then UV cure. Control the UV curing energy to 800mJ / cm 2 , under nitrogen protection, it is cured to form an anti-reflection coating to obtain a highly wear-resistant, anti-glare and anti-reflection optical film.
[0132] The anti-glare coating liquid is the same as that in Example 1.
[0133] Wherein, the anti-reflection coating liquid is prepared by the following method:
[0134] 13 parts by weight of UV curing resin (Guangzhou Songda, SD 1338B), 0.65 parts by weight of DPHA (Sartomer), 4 parts by weight of modified hollow silica dispersion (JGC Catalysts & Chemicals, THRULYA4320, solid content 20%), 0.7 parts by weight of photoinitiator KIP 150, 1 part by weight of fluorinated acrylate modified cage-type polysilsesquioxane, 2 parts by weight of AF additive (China Fluoro Technology, Fluere UV-370), and 300 parts by weight of organic solvent (MIBK) were mixed, stirred at 800 rpm for 1.5 hours, allowed to stand, and defoamed for 12 hours to obtain an anti-reflective optical coating for standby use, with a refractive index of 1.45.
[0135] Comparative Example 1
[0136] A highly wear-resistant, anti-glare and anti-reflection optical film, the preparation method of which comprises the following steps:
[0137] S1. Use a 25# wire rod to evenly coat the anti-glare coating liquid on the surface of the base film (optical grade transparent PET film, thickness of 75μm), bake at 80℃ for 2min, and then UV cure. Control the UV curing energy to 300mJ / cm 2 , forming an anti-glare coating with low water contact, high hardness and high wear resistance;
[0138] S2. Use a 5# wire rod to evenly coat the anti-reflection coating on the anti-glare coating, bake at 80℃ for 2 minutes, and then UV cure. Control the UV curing energy to 800mJ / cm 2 , under nitrogen protection, it is cured to form an anti-reflection coating to obtain a highly wear-resistant, anti-glare and anti-reflection optical film.
[0139] The anti-glare coating liquid is the same as that in Example 1.
[0140] Wherein, the anti-reflection coating liquid is prepared by the following method:
[0141] 11 parts by weight of UV curing resin (Guangzhou Songda, SD 1338B), 5 parts by weight of modified hollow silica dispersion (JGC Catalysts & Chemicals Co., Ltd., THRULYA4320, solid content 20%), 0.7 parts by weight of photoinitiator KIP 150, 0.7 parts by weight of fluorinated acrylate modified cage-type polysilsesquioxane, 2 parts by weight of AF additive (China Fluoro Technology, Fluere UV-370), and an organic solvent (a mixed solvent of 140 parts by weight of MEK and 140 parts by weight of MIBK) were mixed, stirred at 800 rpm for 1.5 hours, allowed to stand, and defoamed for 12 hours to obtain an anti-reflective optical coating for standby use, with a refractive index of 1.45.
[0142] Comparative Example 2
[0143] A highly wear-resistant, anti-glare and anti-reflection optical film, the preparation method of which comprises the following steps:
[0144] S1. Use a 30# wire rod to evenly coat the anti-glare coating liquid on the surface of the base film (optical grade transparent PET film, thickness of 75μm), bake at 80℃ for 2min, and then UV cure. Control the UV curing energy to 300mJ / cm 2 , forming an anti-glare coating with low water contact, high hardness and high wear resistance;
[0145] S2. Use a 5# wire rod to evenly coat the anti-reflection coating on the anti-glare coating, bake at 80℃ for 2 minutes, and then UV cure. Control the UV curing energy to 800mJ / cm 2 , and cured under nitrogen protection to form an anti-reflection coating to obtain the highly wear-resistant, anti-glare, anti-reflection optical film.
[0146] The anti-glare coating liquid is the same as that in Example 1.
[0147] Wherein, the anti-reflection coating liquid is prepared by the following method:
[0148] 12 parts by weight of UV curing resin (Guangzhou Songda, SD 1338B), 0.6 parts by weight of DPHA (Sartomer), 6 parts by weight of modified hollow silica dispersion (JGC Catalysts & Chemicals, THRULYA4320, solid content 20%), 0.7 parts by weight of photoinitiator KIP 150, 2 parts by weight of fluorinated acrylate modified cage-type polysilsesquioxane, 2 parts by weight of AF additive (China Fluoro Technology, Fluere UV-370), and an organic solvent (a mixed solvent of 100 parts by weight of MEK and 150 parts by weight of MIBK) were mixed and stirred for 1.5 hours at a stirring speed of 800 rpm to obtain an anti-reflective optical coating liquid with a refractive index of 1.45. The liquid was allowed to stand and defoamed for 12 hours to obtain an anti-reflective optical coating liquid for standby use with a refractive index of 1.45.
[0149] Comparative Example 3
[0150] The difference between this example and Example 1 is that the solid nano wear-resistant particles FPU-Al are modified with fluorinated acrylate. 2 O 3 / SiO 2 Instead of the fluorinated acrylate-modified cage-type polysilsesquioxane in Example 1.
[0151] Among them, fluorinated acrylate modified solid nano wear-resistant particles FPU-Al 2 O 3 / SiO 2 The film is prepared by the same method as that in Example 1 of the highly wear-resistant, low-color-difference, bendable anti-reflection film and its preparation method in patent CN117700794A.
[0152] This technical solution uses fluorinated acrylate modified cage polysilsesquioxane (FPU-POSS) to replace the fluorinated acrylate modified solid nano wear-resistant particles (FPU-Al 2 O 3 / SiO 2 ), POSS is an organic-inorganic nanoparticle with a three-dimensional structure. The inorganic scaffold structure composed of Si and O can give the hybrid material excellent mechanical properties. In addition, there are 8 organic substituent groups connected to the 8 Si vertices. After molecular design, the solubility of POSS in the organic system can be increased, and the compatibility with the polymer can be improved. More importantly, the FPU-POSS reaction group can realize the chemical bonding between the POSS molecules and the photocurable main resin polymer, further improve the degree of cross-linking, and improve the surface hardness and wear resistance of the coating.
[0153] The main raw materials and proportions of the embodiments and comparative examples are summarized in Table 1 below (the units in the table are parts by weight):
[0154] Table 1
[0155]
[0156] The following performance tests were performed on the membrane products prepared in the examples and comparative examples:
[0157] (1) Refractive index of coating: The coating liquid is applied on the silicon wafer with a coating thickness of 250-500 nm. After drying and light curing, the refractive index of the optical resin is tested using an ellipsometer.
[0158] (2) Reflectivity: Cut the anti-reflection film into 5 cm*5 cm size, stick a black film on the back of the anti-reflection film, use a UV spectrophotometer to test the reflectivity in the reflection mode at a wavelength of 380-780nm, and record the reflectivity of the optical film at 550nm.
[0159] (3) Transmittance and haze: The transmittance and haze of the optical film were measured using a Nippon Denshoku NDH 2000N haze meter using a transmitted light method in accordance with JIS K-7105.
[0160] (4) Water contact angle (WCA): A CA10000 water contact angle tester manufactured by Dongguan Kandi Electronic Equipment Co., Ltd. was used with a 2.0 μL droplet. The optical film was placed face up on the test bench and fixed with tape. The water contact angle was calculated using the measurement method using the test software.
[0161] (5) Pencil hardness: According to JISK-5600 standard, use Elcometer 3086 pencil hardness tester to measure the pencil hardness of optical film. Test method: Use Mitsubishi pencil with hardness of H to 3H to draw 5 lines with a length of 5 cm under a load of 500g, then observe whether the optical film coating is scratched under fluorescent light and judge according to the following standards.
[0162]
Judgment criteria
[0163] 0 to 2 scratches, judged OK
[0164] 3 to 5 scratches, judged as NG
[0165] (6) Abrasion resistance test: Use four layers of dust-free cloth (Canmax TA9008) to wrap the test head (test head size 2*2cm), apply a load of 1000g, and rub back and forth on the surface of the highly wear-resistant anti-glare and anti-reflection optical film at a constant rate (40cycle / min) with a stroke of 40mm. Observe the coating surface for scratches with the naked eye. When the first scratch appears on the surface, record the number of wiping times to characterize the wear resistance. The measuring instrument is Kunshan Jingjia Instrument A20-339 Steel Wool Resistance Tester.
[0166] (7) Anti-glare performance test: The back of the highly wear-resistant anti-glare and anti-reflection optical film is attached to the OCA on a commercially available black acrylic plate, with the front of the highly wear-resistant anti-static anti-glare and anti-reflection optical film facing upward. The anti-glare performance is judged by visually observing the reflected image when irradiated with a three-wavelength fluorescent lamp. The specific standards are as follows: A: The shape of the fluorescent lamp is completely invisible; B: The outline of the fluorescent lamp is vaguely visible; C: The outline of the fluorescent lamp is clearly visible.
[0167] (8) Adhesion of hard coating: Use a grid cutter (1 mm*1 mm) to cut grids on the surface of the hard coating, and then use 3M #600 tape to adhere. According to JIS K5600 standard, use a magnifying glass to observe the shedding of grids.
[0168]
Judgment criteria
[0169] 5B: The cut edges are completely smooth, and there is no peeling on the lattice edges.
[0170] 4B: There is small flakes at the intersection of the cuts, and the damage in the cross-cut area is ≤5%.
[0171] 3B: The edges and / or intersections of the cuts are peeled off, with an area of 5-15%.
[0172] 2B: There is partial or complete peeling along the edge of the cut, and / or part of the grid is completely peeled off. The peeled area is 15-35%.
[0173] 1B: Large pieces of the cut edge peel off / or some squares peel off partially or completely, with an area of 35-65%.
[0174] 0B: Large pieces of the cut edge peel off / or some squares peel off partially or completely, with an area of >65%.
[0175] The test results are shown in Table 2 below:
[0176] Table 2
[0177]
[0178] According to the test results in Table 2, it can be explained that:
[0179] Through the synergistic effect of the components in Examples 1-5 of the present invention, the prepared anti-glare anti-reflection films have high wear resistance and good anti-reflection effect, and have excellent comprehensive performance; through the comparative analysis of Example 1 and Example 2, it can be seen that Example 2 uses active monomers and UV curing resins and other components to synergize, which can increase the degree of crosslinking and improve the wear resistance of the coating surface. Through the comparative analysis of Example 2 and Example 1, it can be seen that the excessive addition of fluorinated acrylate-modified cage-type polysilsesquioxane has large steric hindrance, reduces the crosslinking density, and makes the wear resistance of the coating surface worse. Through the comparative analysis of Example 3 and Example 1, it can be seen that Example 1 uses fluorinated acrylate-modified cage-type polysilsesquioxane to replace the fluorinated acrylate-modified solid nano wear-resistant particles FPU-Al 2 O 3 / SiO 2 , which can realize chemical bonding between POSS molecules and photocurable main resin polymer, improve the degree of cross-linking during the photocuring reaction, and improve the surface hardness and wear resistance of the coating.
[0180] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.
Claims
1. A highly wear-resistant, anti-glare and anti-reflection optical film, characterized in that: The invention comprises a base film, an anti-glare coating formed on the base film, and an anti-reflection coating formed on the anti-glare coating: The anti-reflection coating is obtained by coating an anti-reflection coating liquid and then curing the anti-reflection coating liquid, wherein the anti-reflection coating liquid comprises the following raw material components in parts by weight: 6-24 parts of UV curable resin, 0.3-1.2 parts of active diluent monomer, 2.5-10 parts of modified hollow silica particle dispersion with a solid content of 10-40%, 0.35-1.4 parts of a first photoinitiator, 0.5-1.5 parts of fluorine-containing acrylate modified cage-type polysilsesquioxane, 1-4 parts of AF additive, and 140-560 parts of a first organic solvent.
2. The highly wear-resistant, anti-glare and anti-reflection optical film according to claim 1, characterized in that: The fluorinated acrylate modified cage-type polysilsesquioxane is prepared by the following method: 1-1) under nitrogen protection and light-proof conditions, isophorone diisocyanate, acrylate and a catalyst are mixed, heated and stirred to obtain isocyanate-modified acrylate; 1-2) mixing isocyanate-modified acrylate, hydroxyl fluorinated acrylate and catalyst, heating for reaction, adding pentaerythritol triacrylate for dilution after the reaction, and removing the solvent in the product by vacuum distillation to obtain double-bond terminated fluorinated acrylate: FPU; 1-3) (3-mercaptopropyl)trimethoxysilane is dissolved in methanol, hydrochloric acid is added dropwise while stirring, and the mixture is condensed and refluxed under heating. After the reaction is completed, the mixture is cooled and separated, and the upper clear liquid is discarded. A solvent is added to the remaining product to dissolve the mixture, and the resulting mixture is added to a methanol solvent for precipitation. After standing, the upper clear liquid is discarded, and the lower layer is the product, which is dried in vacuo to obtain the product octamercapto cage-type polysilsesquioxane: POSS-SH; 1-4) Grafting FPU onto the thiol group of POSS-SH by click reaction: POSS-SH is dissolved in a solvent, and FPU and 2,2-dihydroxymethylpropionic acid photoinitiator are added, and the mixture is stirred until it is completely dissolved, irradiated with ultraviolet light, and then the solvent is removed by rotary evaporation. After vacuum drying, the product fluorinated acrylate modified cage-type polysilsesquioxane: FPU-POSS is obtained.
3. The highly wear-resistant, anti-glare and anti-reflection optical film according to claim 2, characterized in that: The fluorinated acrylate modified cage-type polysilsesquioxane is prepared by the following method: 1-1) Under nitrogen protection and light-proof conditions, 100-120 g of isophorone diisocyanate and 0.04-0.06 g of dibutyltin dilaurate as a catalyst are added to a reaction vessel, the temperature is raised to 35-45° C., and then 55-70 g of acrylate is added dropwise to the reaction vessel, and the reaction is stirred at 45-50° C. The reaction endpoint is monitored by measuring the NCO value, and the reaction is terminated when the NCO value is 48-55%. After the reaction is completed, isocyanate-modified acrylate is obtained; 1-2) the isocyanate-modified acrylate and the hydroxyl fluorinated acrylate prepared in step 1-1) are mixed in a molar ratio of 1.1:1, 0.0025-0.01 g of dibutyltin dilaurate as a catalyst is added dropwise while stirring, and the reaction is stirred at 40-60° C. for 1-2 h, and the reaction endpoint is monitored by measuring the NCO value. When the NCO value is less than 0.5%, the reaction is terminated. After the reaction is completed, pentaerythritol triacrylate is added for dilution, and the solvent in the product is removed by vacuum distillation to obtain a double-bond terminated fluorinated acrylate: FPU; 1-3) 9.8 g (3-mercaptopropyl) trimethoxysilane was dissolved in methanol, and 30 mL of concentrated hydrochloric acid with a mass concentration of 36-38% was added dropwise while stirring, and the mixture was condensed and refluxed at 80-100° C. for 12-36 h. After the reaction was completed, the mixture was cooled and layered, and the supernatant was discarded. Dichloromethane was added to the remaining product to dissolve the mixture, and the mixture was added to methanol solvent for precipitation. After standing for 3-5 h, the supernatant was discarded, and the lower layer was the product, which was vacuum dried at 50-70° C. for 4-16 h to obtain the product octamercapto cage-type polysilsesquioxane: POSS-SH; 1-4) Grafting FPU on the thiol group of POSS-SH by click reaction: 1-2g POSS-SH is added to 60-250mL tetrahydrofuran solvent, and 10-20g FPU and 0.25-1g 2,2-dihydroxymethylpropionic acid (DMPA) photoinitiator are added, and magnetic stirring is performed until the mixture is completely dissolved, and ultraviolet light is irradiated for 15-60min, and then the tetrahydrofuran solvent is removed by rotary evaporation at 40-60°C, and vacuum drying is performed at 50-70°C for 4-16h to obtain the product fluorinated acrylate modified cage-type polysilsesquioxane: FPU-POSS.
4. The highly wear-resistant, anti-glare and anti-reflection optical film according to claim 1, characterized in that: The UV curable resin is one or more of fluorocarbon modified polyurethane acrylate, fluorosilicone modified polyurethane acrylate, fluorocarbon modified polyester acrylate, and fluorosilicone modified polyester acrylate; The active monomer is one or more of pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol pentaacrylate and dipentaerythritol hexaacrylate; The first photoinitiator is one or more of 184, 1173, TPO, KIP 150, 160, and Esacure ONE; The AF auxiliary agent is a fluorine-containing acrylate compound; The first organic solvent is one or more of propylene glycol methyl ether, methyl isobutyl ketone, ethyl acetate and butanone.
5. The highly wear-resistant, anti-glare and anti-reflection optical film according to claim 1, characterized in that: The anti-reflection coating liquid is prepared by the following method: UV curable resin, active diluent monomer, modified hollow silica particles, a first photoinitiator, fluorine-containing acrylate modified cage-type polysilsesquioxane, AF auxiliary agent, and a first organic solvent are uniformly mixed to obtain the anti-reflection coating liquid.
6. The highly wear-resistant, anti-glare and anti-reflection optical film according to claim 1, characterized in that: The anti-glare coating is obtained by coating an anti-glare coating liquid and then curing it. The anti-glare coating liquid includes the following raw material components in parts by weight: 1.35-5.4 parts of anti-glare micron particles, 0.4-1.6 parts of a dispersant, 35-150 parts of a second organic solvent, 17.5-70 parts of a high-hardness and high-wear-resistant resin, 4-16 parts of a dual-curing resin, 1-4 parts of a second photoinitiator, and 0.1-0.4 parts of a leveling agent.
7. The highly wear-resistant, anti-glare and anti-reflection optical film according to claim 6, characterized in that: The anti-glare coating liquid is prepared by the following method: 2-1) mixing the anti-glare micron particles, the dispersant and the second organic solvent, and stirring at 800-3200 r / min for 2-8 hours to obtain an anti-glare base coating slurry; 2-2) mixing a high-hardness and high-wear-resistant resin, a dual-curing resin, a second photoinitiator, and a second organic solvent, and stirring at 450-1800 r / min for 30-120 min to obtain an anti-glare base coating clear liquid; 2-3) The anti-glare base coating slurry and the anti-glare base coating clear liquid are mixed, and then a leveling agent is added. After stirring evenly, the mixture is allowed to stand for defoaming for 15-60 minutes to obtain the anti-glare coating liquid.
8. The highly wear-resistant, anti-glare and anti-reflection optical film according to claim 6, characterized in that: The anti-glare micron particles are one or two of modified silica particles and modified PMMA particles; The dispersant is one or more of modified polyacrylate, acrylic block copolymer, and modified polyurethane; The high-hardness and high-wear-resistant resin is polyurethane acrylate, with a functionality of 6-9 and a viscosity of 800-5000 mPa·s; The dual-cure resin is polyurethane-modified acrylic epoxy monoester, with a functionality of 6-9 and a viscosity of 500-5000 mPa·s; The second photoinitiator is one or more of 184, 1173, TPO, KIP 150, 160, and Esacure ONE; The second organic solvent is one or more of propylene glycol methyl ether, methyl isobutyl ketone, ethyl acetate, and butanone.
9. The highly wear-resistant, anti-glare and anti-reflection optical film according to claim 1, characterized in that: The base film is a PET film, a PC film or a TAC film, and has a thickness of 40-100 μm.
10. A method for preparing a highly wear-resistant, anti-glare and anti-reflection optical film according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1. Apply the anti-glare coating evenly on the surface of the base film, bake at 80-100℃ for 1-4min, and then UV cure. Control the UV curing energy to 300-500mJ / cm 2 , forming an anti-glare coating; S2. Evenly apply the anti-reflection coating on the anti-glare coating, bake at 80-100℃ for 1-4min, and then UV cure. Control the UV curing energy to 600-800mJ / cm 2 , forming an anti-reflection coating to obtain the highly wear-resistant, anti-glare anti-reflection optical film.
Citation Information
Cited By
Optical film with anti-dazzle self-repairing function
CN122037267A