High-wear-resistance rubber and preparation method thereof
By combining nitrile rubber with modified styrene butadiene rubber, adding zirconium dioxide and aramid fiber carbon black, and using accelerator and silane coupling agent, the problem of insufficient wear resistance of rubber materials is solved, significantly improving the rubber Wear resistance and service life.
Patent Information
- Application Number
- CN202410991530.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
The existing rubber materials are severely worn after long-term use, which affects their service life and performance stability, and lacks wear resistance.
Using the preparation method of high wear-resistant rubber, nitrile rubber and modified styrene-butadiene rubber as matrix, zirconium dioxide as filler, and aramid fiber and carbon black are added to the surface of the styrene-butadiene rubber, and accelerators and silane couples are used. Coupling agents and plasticizers can improve the vulcanization efficiency and filler dispersion of rubber, reduce mixing energy consumption, and enhance the wear resistance of rubber.
It significantly improves the wear resistance and tensile strength of rubber, reduces agglomeration, enhances the interface compatibility between fillers and rubber matrix, and extends the service life of rubber.
Smart Images

Figure BDA0004959000810000061 
Figure BDA0004959000810000071
Abstract
Description
Technical Field
[0001] The invention relates to the field of rubber, in particular to a highly wear-resistant rubber and a preparation method thereof. Background Art
[0002] As an important material widely used in many fields such as industry, transportation, and daily life, rubber has good physical and chemical properties. Its wear resistance is a key factor in measuring its quality and service life. It plays an important role in many fields such as tires, seals, and conveyor belts.
[0003] However, although there are many types of rubber materials on the market, they are often severely worn after long-term use, which affects their service life and performance stability. Therefore, their wear resistance still needs to be improved. Summary of the invention
[0004] In order to improve the wear resistance of rubber, the present application provides a high wear-resistant rubber and a preparation method thereof.
[0005] In the first aspect, the present application provides a highly wear-resistant rubber using the following technical solution: A highly wear-resistant rubber comprises the following raw materials in parts by weight: 30-60 parts of nitrile rubber; 40-70 parts of modified styrene-butadiene rubber; 30-70 parts of zirconium dioxide; 2-6 parts of accelerator; 5-15 parts of silane coupling agent; 2-4 parts of plasticizer; and 1-3 parts of antioxidant. The modified styrene-butadiene rubber is modified from the following raw materials: styrene-butadiene rubber, deionized water, potassium oleate, aramid fiber and carbon black.
[0006] By adopting the above technical scheme, the present application mixes nitrile rubber and modified styrene butadiene rubber as the rubber matrix, and zirconium dioxide has high wear resistance and is added to the nitrile rubber and modified styrene butadiene rubber as a filler; at the same time, the present application modifies the styrene butadiene rubber, and adds aramid fiber and carbon black to the surface of the styrene butadiene rubber, so that the filler can be better dispersed in the rubber matrix, reduce agglomeration, and further improve the tensile strength of the rubber; the accelerator improves the vulcanization efficiency during the vulcanization process of the rubber, the silane coupling agent can improve the interface compatibility between the filler and the rubber matrix, and further improve the dispersibility of zirconium dioxide, and the plasticizer can reduce the energy consumption during rubber mixing, thereby better improving the wear resistance of the rubber.
[0007] Preferably, the preparation method of the modified styrene butadiene rubber is: after ultrasonically dispersing 10-30 parts by weight of deionized water and 2-6 parts by weight of potassium oleate, 5-15 parts by weight of aramid fiber are added and mixed, after suction filtration and drying, 40-60 parts by weight of styrene butadiene rubber and 20-40 parts by weight of carbon black are stirred evenly and then kneaded to obtain the modified styrene butadiene rubber.
[0008] By adopting the above-mentioned technical scheme, the present application uses deionized water, potassium oleate, aramid fiber and carbon black to modify styrene-butadiene rubber, and the aramid fiber and styrene-butadiene rubber are mechanically interlocked through potassium oleate and carbon black, so that the carbon black has better dispersibility and interface bonding ability in styrene-butadiene rubber, thereby improving the tensile strength and wear resistance of the rubber.
[0009] Preferably, the weight ratio of potassium oleate, aramid fiber, styrene-butadiene rubber and carbon black is (0.48-0.58):1:(5.2-5.6):(2.2-2.7).
[0010] By adopting the above technical scheme, when potassium oleate, aramid fiber, styrene butadiene rubber and carbon black are in a specific weight ratio, the four are mixed to produce a synergistic effect. The carbon black and aramid fiber are combined to improve the wear resistance and mechanical strength of the styrene butadiene rubber. Potassium oleate, as a surfactant, can reduce the viscosity of the styrene butadiene rubber, making the rubber easier to mix with the aramid fiber and carbon black, thereby improving the corrosion resistance and wear resistance of the rubber.
[0011] Preferably, the zirconium dioxide is modified zirconium dioxide, and the preparation method of the modified zirconium dioxide is: after reacting 10-20 parts by weight of zirconium dioxide with 5-10 parts by weight of nitric acid, 5-15 parts by weight of dichloromethane and 2-8 parts by weight of thionyl chloride are added and mixed and stirred, and then 10-30 parts by weight of N,N-dimethylformamide and 15-25 parts by weight of β-cyclodextrin are added and stirred for reaction, and then washed and dried to obtain the modified zirconium dioxide.
[0012] By adopting the above technical scheme, the present application modifies zirconium dioxide, performs surface chlorination with thionyl chloride, and then grafts it with β-cyclodextrin. β-cyclodextrin has a special inclusion complex and forms an inclusion complex on the surface of zirconium dioxide, thereby increasing the reaction activity of the zirconium dioxide surface and allowing zirconium dioxide to be better dispersed in the rubber component, thereby significantly improving the wear resistance of the rubber.
[0013] Preferably, the weight ratio of the zirconium dioxide, thionyl chloride and β-cyclodextrin is (3.2-3.6):1:(3.6-4.8).
[0014] By adopting the above technical scheme, when zirconium dioxide, thionyl chloride and β-cyclodextrin are in a specific weight ratio, thionyl chloride and β-cyclodextrin are grafted on the surface of zirconium dioxide after reaction, so that the compatibility of zirconium dioxide and rubber is improved, and zirconium dioxide is evenly dispersed in the rubber component as a filler, thereby improving the wear resistance and chemical stability of the rubber.
[0015] Preferably, the accelerator comprises one of methylenebenzene dithiocarbamate and zinc diphenyl dithiocarbamate.
[0016] By adopting the above technical solution and selecting a suitable accelerator, the present application can shorten the vulcanization time, improve the vulcanization efficiency, and improve the wear resistance of the rubber.
[0017] Preferably, the weight ratio of the nitrile rubber, the modified styrene butadiene rubber and the modified zirconium dioxide is (0.96-1.1):1:(0.9-1.08).
[0018] By adopting the above technical scheme, when nitrile rubber, modified styrene-butadiene rubber and modified zirconium dioxide are in a specific weight ratio, the three work together to produce a synergistic effect. The modified zirconium dioxide after surface treatment can improve the compatibility and dispersibility with the rubber matrix, help to evenly bear stress, and further improve the wear resistance and tensile strength of the rubber; at the same time, the three can be mixed to further improve the corrosion resistance of the rubber.
[0019] Preferably, the plasticizer includes one of dioctyl phthalate and dioctyl adipate.
[0020] By adopting the above technical solution and selecting a suitable plasticizer, the processing performance of the rubber can be improved, the rubber viscosity and the energy consumption during mixing can be reduced, thereby increasing the tensile strength of the rubber.
[0021] Preferably, the antioxidant includes antioxidant 1010 and antioxidant 168.
[0022] By adopting the above technical solution, the antioxidant can protect the rubber from aging and performance degradation caused by oxidation.
[0023] In a second aspect, the present application provides a method for preparing a highly wear-resistant rubber using the following technical solution: A method for preparing highly wear-resistant rubber comprises the following steps: mixing and kneading nitrile rubber, modified styrene-butadiene rubber, silane coupling agent and plasticizer, adding zirconium dioxide, accelerator and antioxidant and continuing kneading, thinning and cutting after cooling, and obtaining the highly wear-resistant rubber after vulcanization.
[0024] By adopting the above technical scheme, rubber with excellent wear resistance can be prepared by simply mixing the components.
[0025] In summary, this application has the following beneficial technical effects: 1. The present application mixes nitrile rubber and modified styrene butadiene rubber as a rubber matrix, and zirconium dioxide has high wear resistance and is added to the nitrile rubber and modified styrene butadiene rubber as a filler; at the same time, the present application modifies the styrene butadiene rubber, and adds aramid fiber and carbon black on the surface of the styrene butadiene rubber, so that the filler can be better dispersed in the rubber matrix, reduce agglomeration, and further improve the mechanical strength of the rubber; the accelerator improves the vulcanization efficiency during the vulcanization process of the rubber, the silane coupling agent can improve the interface compatibility between the filler and the rubber matrix, and further improve the dispersibility of zirconium dioxide, and the plasticizer can reduce the energy consumption during rubber mixing, thereby better improving the wear resistance of the rubber.
[0026] 2. When potassium oleate, aramid fiber, styrene butadiene rubber and carbon black are in a specific weight ratio, the four mix to produce a synergistic effect. The carbon black and aramid fiber combine to improve the wear resistance and mechanical strength of styrene butadiene rubber. Potassium oleate, as a surfactant, can reduce the viscosity of styrene butadiene rubber, making the rubber easier to mix with aramid fiber and carbon black, thereby improving the corrosion resistance and wear resistance of the rubber. DETAILED DESCRIPTION
[0027] The present application is further described in detail below in conjunction with embodiments and comparative examples. Example
[0028] Example 1 A method for preparing a highly wear-resistant rubber comprises the following steps: putting 30g of nitrile rubber, 40g of modified styrene-butadiene rubber, 5g of KH560 silane coupling agent and 2g of plasticizer into an open mill, mixing and kneading for 30min at a speed of 120r / min and a temperature of 70°C, then adding 30g of zirconium dioxide, 2g of accelerator and 1g of antioxidant, raising the temperature to 80°C, and continuing to knead for 20min at a speed of 150r / min, cooling to 50°C, thinning and cutting, transferring to a flat vulcanizer and vulcanizing for 60min to obtain the highly wear-resistant rubber.
[0029] The accelerator is methylene benzene dithiocarbamate, the plasticizer is dioctyl phthalate, the antioxidant is antioxidant 1010; the nitrile rubber is selected from Eni NBR-N3980; the styrene butadiene rubber is selected from Kraton of the United States, with the brand number D1107JSP.
[0030] The preparation method of the modified styrene-butadiene rubber is as follows: 10g of deionized water and 2g of potassium oleate are ultrasonically dispersed for 20min at an ultrasonic frequency of 1000Hz, and then 5g of aramid fiber is added to a magnetic stirrer, mixed and stirred for 2h at a temperature of 80°C and a speed of 60r / min, filtered and dried at a temperature of 80°C, and then mixed with 40g of styrene-butadiene rubber and 20g of carbon black at a speed of 90r / min for 30s and then discharged to obtain the modified styrene-butadiene rubber. The aramid fiber is purchased from Shuobang New Materials, and the elongation is 2.5%.
[0031] Example 2 A method for preparing a highly wear-resistant rubber comprises the following steps: putting 60g of nitrile rubber, 70g of modified styrene-butadiene rubber, 15g of KH560 silane coupling agent and 4g of plasticizer into an open mill, mixing and kneading for 30min at a speed of 120r / min and a temperature of 70°C, then adding 70g of zirconium dioxide, 6g of accelerator and 3g of antioxidant, raising the temperature to 80°C, and continuing to knead for 20min at a speed of 150r / min, cooling to 50°C, thinning and cutting, transferring to a flat vulcanizer and vulcanizing for 60min to obtain the highly wear-resistant rubber.
[0032] The accelerator is zinc diphenyl disulfide carbamate, the plasticizer is dioctyl adipate, and the antioxidant is antioxidant 168; the nitrile rubber is selected from Eni NBR-N3980; the styrene-butadiene rubber is selected from Kraton of the United States, with the brand number D1107JSP.
[0033] The preparation method of the modified styrene-butadiene rubber is as follows: 10g of deionized water and 2g of potassium oleate are ultrasonically dispersed for 20min at an ultrasonic frequency of 1000Hz, and then 5g of aramid fiber is added to a magnetic stirrer, mixed and stirred for 2h at a temperature of 80°C and a speed of 60r / min, filtered and dried at a temperature of 80°C, and then mixed with 40g of styrene-butadiene rubber and 20g of carbon black at a speed of 90r / min for 30s and then discharged to obtain the modified styrene-butadiene rubber. The aramid fiber is purchased from Shuobang New Materials, and the elongation is 2.5%.
[0034] Example 3 A method for preparing a highly wear-resistant rubber comprises the following steps: putting 45g of nitrile rubber, 55g of modified styrene-butadiene rubber, 10g of KH560 silane coupling agent and 3g of plasticizer into an open mill, mixing and kneading for 30min at a speed of 120r / min and a temperature of 70°C, then adding 50g of zirconium dioxide, 4g of an accelerator and 2g of an antioxidant, raising the temperature to 80°C, and continuing to knead for 20min at a speed of 150r / min, cooling to 50°C, thinning the sheets, transferring the sheets to a flat vulcanizer and vulcanizing for 60min to obtain the highly wear-resistant rubber.
[0035] The accelerator is methylene benzene dithiocarbamate, the plasticizer is dioctyl phthalate, the antioxidant is antioxidant 1010; the nitrile rubber is selected from Eni NBR-N3980; the styrene butadiene rubber is selected from Kraton of the United States, with the brand number D1107JSP.
[0036] The preparation method of the modified styrene-butadiene rubber is as follows: 10g of deionized water and 2g of potassium oleate are ultrasonically dispersed for 20min at an ultrasonic frequency of 1000Hz, and then 5g of aramid fiber is added to a magnetic stirrer, mixed and stirred for 2h at a temperature of 80°C and a speed of 60r / min, filtered and dried at a temperature of 80°C, and then mixed with 40g of styrene-butadiene rubber and 20g of carbon black at a speed of 90r / min for 30s and then discharged to obtain the modified styrene-butadiene rubber. The aramid fiber is purchased from Shuobang New Materials, and the elongation is 2.5%.
[0037] Example 4 A method for preparing highly wear-resistant rubber, which is different from Example 3 in that: the preparation method of modified styrene-butadiene rubber is as follows: 30g of deionized water and 6g of potassium oleate are ultrasonically dispersed at an ultrasonic frequency of 1000 Hz for 20 minutes, 15g of aramid fiber is added in a magnetic stirrer, and mixed and stirred for 2 hours at a temperature of 80°C and a speed of 60r / min, filtered and dried at a temperature of 80°C, and then stirred evenly with 60g of styrene-butadiene rubber and 40g of carbon black at a speed of 90r / min for 30 seconds, and then the modified styrene-butadiene rubber is obtained.
[0038] Example 5 A method for preparing highly wear-resistant rubber, which is different from Example 3 in that: the input amount of potassium oleate is 4.8g, the input amount of aramid fiber is 10g, the input amount of styrene-butadiene rubber is 52g, and the input amount of carbon black is 22g.
[0039] Example 6 A method for preparing highly wear-resistant rubber, which is different from Example 3 in that: the input amount of potassium oleate is 5.8g, the input amount of aramid fiber is 10g, the input amount of styrene-butadiene rubber is 56g, and the input amount of carbon black is 27g.
[0040] Example 7 A method for preparing highly wear-resistant rubber, which is different from Example 6 in that an equal amount of zirconium dioxide is replaced with modified zirconium dioxide. The preparation method of the modified zirconium dioxide is as follows: 10g of zirconium dioxide is reacted with 5g of nitric acid, and then 5g of dichloromethane and 2g of thionyl chloride are added and stirred for 1h, and then 10g of N,N-dimethylformamide and 15g of β-cyclodextrin are added and stirred for 2h, and then the mixture is washed with water and dried at 80°C for 2h to obtain modified zirconium dioxide.
[0041] Example 8 A method for preparing highly wear-resistant rubber, which is different from Example 6 in that an equal amount of zirconium dioxide is replaced with modified zirconium dioxide. The preparation method of the modified zirconium dioxide is as follows: 20g of zirconium dioxide is reacted with 10g of nitric acid, and then 15g of dichloromethane and 8g of thionyl chloride are added and stirred for 1h, and then 30g of N,N-dimethylformamide and 25g of β-cyclodextrin are added and stirred for 2h, and then the mixture is washed with water and dried at 80°C for 2h to obtain modified zirconium dioxide.
[0042] Example 9 A method for preparing highly wear-resistant rubber, which is different from Example 8 in that: the input amount of zirconium dioxide is 16g, the input amount of thionyl chloride is 5g, and the input amount of β-cyclodextrin is 18g.
[0043] Example 10 A method for preparing highly wear-resistant rubber, which is different from Example 8 in that: the input amount of zirconium dioxide is 18g, the input amount of thionyl chloride is 5g, and the input amount of β-cyclodextrin is 24g.
[0044] Embodiment 11 A method for preparing highly wear-resistant rubber, which is different from Example 10 in that the input amount of nitrile rubber is 48g, the input amount of modified styrene butadiene rubber is 50g, and the input amount of modified zirconium dioxide is 45g.
[0045] Example 12 A method for preparing highly wear-resistant rubber, which is different from Example 10 in that the input amount of nitrile rubber is 55g, the input amount of modified styrene butadiene rubber is 50g, and the input amount of modified zirconium dioxide is 54g.
[0046] Comparative Example Comparative Example 1 A method for preparing highly wear-resistant rubber, which is different from Example 3 in that an equal amount of modified styrene-butadiene rubber is replaced with styrene-butadiene rubber.
[0047] Comparative Example 2 A method for preparing highly wear-resistant rubber, which is different from Example 3 in that an equal amount of nitrile rubber is replaced by modified styrene-butadiene rubber.
[0048] Comparative Example 3 A method for preparing highly wear-resistant rubber, which is different from Example 3 in that an equal amount of modified styrene-butadiene rubber is replaced by cis-1,1-dione rubber.
[0049] Comparative Example 4 A method for preparing highly wear-resistant rubber, which is different from Example 3 in that an equal amount of zirconium dioxide is replaced by silicon dioxide.
[0050] Performance testing: Wear resistance test: Referring to GBT1689-1998 wear resistance of vulcanized rubber, the rubbers prepared in Examples 1-12 and Comparative Examples 1-4 were tested using an Akron abrasion machine; Tensile strength test: The rubbers prepared in Examples 1-12 and Comparative Examples 1-4 were subjected to a tensile property test (25°C) according to standard GB / T 528-2009, and then the rubbers were subjected to an alkaline corrosion condition of 20 wt% sodium hydroxide solution at 90°C for 72 h and then the tensile strength was tested again.
[0051] According to the data comparison of Examples 1-3 and Comparative Examples 1-4, the present application mixes nitrile rubber and modified styrene butadiene rubber as the rubber matrix, and zirconium dioxide has high wear resistance and is added to the nitrile rubber and modified styrene butadiene rubber as a filler; at the same time, the present application modifies the styrene butadiene rubber, and adds aramid fiber and carbon black to the surface of the styrene butadiene rubber, so that the filler can be better dispersed in the rubber matrix, reduce agglomeration, and further improve the mechanical strength of the rubber; the accelerator improves the vulcanization efficiency during the vulcanization process of the rubber, the silane coupling agent can improve the interface compatibility between the filler and the rubber matrix, and further improve the dispersibility of zirconium dioxide, and the plasticizer can reduce the energy consumption during rubber mixing, thereby better improving the wear resistance of the rubber.
[0052] According to the data comparison of Examples 3-6, it can be obtained that when potassium oleate, aramid fiber, styrene-butadiene rubber and carbon black are in a specific weight ratio, the four are mixed to produce a synergistic effect. The carbon black and aramid fiber are combined to improve the wear resistance and mechanical strength of the styrene-butadiene rubber. Potassium oleate, as a surfactant, can reduce the viscosity of the styrene-butadiene rubber, making the rubber easier to mix with the aramid fiber and carbon black, thereby improving the corrosion resistance and wear resistance of the rubber.
[0053] According to the data comparison of Examples 6-8, the present application modifies zirconium dioxide, performs surface chlorination with thionyl chloride, and then grafts it with β-cyclodextrin. β-cyclodextrin has a special inclusion complex and forms an inclusion compound on the surface of zirconium dioxide, thereby increasing the reaction activity of the zirconium dioxide surface and allowing zirconium dioxide to be better dispersed in the rubber component, thereby significantly improving the wear resistance of the rubber.
[0054] According to the data comparison of Examples 8-10, it can be obtained that when zirconium dioxide, thionyl chloride and β-cyclodextrin are in a specific weight ratio, thionyl chloride and β-cyclodextrin are grafted on the surface of zirconium dioxide after reaction, so that the compatibility of zirconium dioxide and rubber is improved, and zirconium dioxide is uniformly dispersed in the rubber component as a filler, thereby improving the wear resistance and chemical stability of the rubber.
[0055] According to the data comparison of Examples 10-12, when nitrile rubber, modified styrene-butadiene rubber and modified zirconium dioxide are in a specific weight ratio, the three work together to produce a synergistic effect. The modified zirconium dioxide after surface treatment can improve the compatibility and dispersibility with the rubber matrix, help to evenly bear stress, and further improve the wear resistance and tensile strength of the rubber; at the same time, the three can be mixed to further improve the corrosion resistance of the rubber.
Claims
1. A highly wear-resistant rubber, characterized in that: The invention comprises the following raw materials in parts by weight: 30-60 parts of nitrile rubber; 40-70 parts of modified styrene-butadiene rubber; 30-70 parts of zirconium dioxide; 2-6 parts of accelerator; 5-15 parts of silane coupling agent; 2-4 parts of plasticizer; 1-3 parts of antioxidant; the modified styrene-butadiene rubber is modified by the following raw materials: Styrene butadiene rubber, deionized water, potassium oleate, aramid fiber and carbon black.
2. A highly wear-resistant rubber according to claim 1, characterized in that: The preparation method of the modified styrene butadiene rubber is as follows: 10-30 parts by weight of deionized water and 2-6 parts by weight of potassium oleate are ultrasonically dispersed, 5-15 parts by weight of aramid fiber are added and mixed, filtered and dried, and then mixed with 40-60 parts by weight of styrene butadiene rubber and 20-40 parts by weight of carbon black to obtain the modified styrene butadiene rubber.
3. A highly wear-resistant rubber according to claim 2, characterized in that: The weight ratio of potassium oleate, aramid fiber, styrene-butadiene rubber and carbon black is (0.48-0.58):1:(5.2-5.6):(2.2-2.7).
4. The highly wear-resistant rubber according to claim 1, characterized in that: The zirconium dioxide is modified zirconium dioxide. The preparation method of the modified zirconium dioxide is as follows: 10-20 parts by weight of zirconium dioxide and 5-10 parts by weight of nitric acid are reacted, and then 5-15 parts by weight of dichloromethane and 2-8 parts by weight of thionyl chloride are added and mixed and stirred, and then 10-30 parts by weight of N,N-dimethylformamide and 15-25 parts by weight of beta-cyclodextrin are added and stirred for reaction, and then washed and dried to obtain the modified zirconium dioxide.
5. The highly wear-resistant rubber according to claim 4, characterized in that: The weight ratio of the zirconium dioxide, thionyl chloride and beta-cyclodextrin is (3.2-3.6):1:(3.6-4.8).
6. The highly wear-resistant rubber according to claim 1, characterized in that: The accelerator includes one of methylenebenzene dithiocarbamate and zinc diphenyl dithiocarbamate.
7. The highly wear-resistant rubber according to claim 4, characterized in that: The weight ratio of the nitrile rubber, the modified styrene butadiene rubber and the modified zirconium dioxide is (0.96-1.1):1:(0.9-1.08).
8. The highly wear-resistant rubber according to claim 1, characterized in that: The plasticizer includes one of dioctyl phthalate and dioctyl adipate.
9. The highly wear-resistant rubber according to claim 1, characterized in that: The antioxidants include antioxidant 1010 and antioxidant 168 .
10. A method for preparing highly wear-resistant rubber, characterized in that: The method for preparing the highly wear-resistant rubber according to any one of claims 1 to 9 comprises the following steps: mixing and kneading nitrile rubber, modified styrene-butadiene rubber, silane coupling agent and plasticizer, adding zirconium dioxide, accelerator and antioxidant and continuing to knead, thinning and sheeting after cooling, and obtaining the highly wear-resistant rubber after vulcanization.