Power cable material for oil-resistant oil drilling platform and preparation method thereof
By using modified white carbon black and additives in cable materials to form a hybrid crosslinking network structure, the problem of insufficient swelling and wear resistance in oily media is solved, and high-performance wear resistance and flame retardant are achieved and hydrophobic and oleophobic effects, extending service life.
Patent Information
- Application Number
- CN202411096633.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-12
AI Technical Summary
Existing cable materials will swell when they come into contact with oil medium for a long time, resulting in reduced strength and mechanical properties. They will face frequent dragging and friction during the use of oil drilling platforms, resulting in insufficient wear resistance and inability to effectively deal with complex use. Working conditions.
Using a cable material including ethylene propylene rubber, modified white carbon black, additives and other components, the hybrid crosslinking network structure is formed through the esterification reaction of modified white carbon black and the chemical action of additives to improve the cable The mechanical strength, wear resistance and flame retardant properties of the material, and improve the hydrolipophobic properties through fluorine atoms and halogen-free flame retardant elements in the additive.
It significantly improves the wear resistance, flame retardancy, hydrophobic oleophobicity and insulation of cable materials, extends the service life, and avoids aging, cracking and leakage problems at high temperatures.
Smart Images

Figure BDA0004988116600000021 
Figure BDA0004988116600000031 
Figure BDA0004988116600000032
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cable materials, and in particular, relates to a power cable material for an oil-resistant petroleum drilling platform and a preparation method thereof. Background Art
[0002] In recent years, with the growth of the national economy and the development of the cable industry, the use of cables in my country has increased.
[0003] With the frequent occurrence of fire accidents, people's awareness of fire safety has been strengthened, and the flame retardant problem of wires and cables has gradually attracted everyone's attention. If rubber products are in contact with oil media for a long time during use, the oil can penetrate into the rubber and cause it to swell, resulting in a decrease in the strength and other mechanical properties of the rubber. The reason why oil can cause rubber to swell is that after the oil penetrates into the rubber, the molecules diffuse with each other, causing the network structure of the vulcanized rubber to change. In addition, due to frequent operating requirements, in actual use, it will be frequently dragged on the oil extraction platform. During this process, the cable material is frequently exposed to friction with the ground.
[0004] Therefore, for power cable materials for oil drilling platforms, how to develop a rubber cable material that is flame retardant, oil resistant and wear resistant to cope with complex operating conditions and ensure a longer service life of the product is one of the technical challenges faced by technical personnel in this field. Summary of the invention
[0005] The purpose of the present invention is to overcome the defects of the prior art and provide an oil-resistant power cable material for oil drilling platforms and a preparation method thereof.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] A power cable material for an oil-resistant oil drilling platform comprises the following raw materials in parts by weight: 70-80 parts of EPDM rubber, 20-30 parts of hydrogenated nitrile rubber, 8-12 parts of chloroprene rubber, 15-25 parts of modified white carbon black, 10-15 parts of additives, 1.8-2.4 parts of antioxidants, 0.8-1.2 parts of antioxidants, 0.8-1.2 parts of ultraviolet absorbers, and 0.5-1 parts of initiators.
[0008] Furthermore, the modified silica is prepared by the following steps:
[0009] Add white carbon black and acetone to a three-necked flask, add maleic anhydride and DMAP (4-dimethylaminopyridine) while stirring, stir and heat to 50°C after adding, keep warm for 12 hours, filter after the reaction, wash with deionized water 3 times, wash with anhydrous ethanol 3 times, dry at 80°C for 12 hours to obtain modified white carbon black. The mass ratio of white carbon black to maleic anhydride is 8:1.
[0010] There are abundant hydroxyl groups on the surface of silica. Under the catalytic action of DMAP, the hydroxyl groups on the surface of silica can undergo esterification reaction with succinic anhydride. The reaction process is as follows:
[0011]
[0012] White carbon black can improve the density and wear resistance of cable materials, and at the same time increase the mechanical strength and pressure resistance of cable materials, thereby increasing the service life of cables; the high specific surface area and structural characteristics of white carbon black can effectively absorb and disperse heat, thereby improving the heat resistance of cables and avoiding aging, cracking, leakage and other problems caused by insufficient heat resistance.
[0013] The surface of modified silica contains abundant carbon-carbon double bonds, which can produce chemical reaction with the carbon-carbon double bonds of the side chain of EPDM rubber under the action of initiator, and can also produce chemical reaction with the carbon-carbon double bonds at the end of the auxiliary agent under the action of initiator. Therefore, modified silica can be uniformly dispersed and stably present in the cable material, and at the same time, it forms a hybrid cross-linked network structure with the auxiliary agent and EPDM rubber, which further improves the wear resistance, mechanical strength and heat resistance of the cable material of the present invention, and these properties are durable and stable.
[0014] Furthermore, the auxiliary agent is prepared by the following steps:
[0015] S1. Add 2-amino-4,6-dichloro-1,3,5-triazine, triethylamine and DMSO (dimethyl sulfoxide) to a dry brown three-necked flask under nitrogen protection, stir until completely dissolved, then slowly add diallylamine, control the temperature at 0-5°C to react for 8 hours after the addition is complete, distill under reduced pressure after the reaction is completed, purify by column chromatography (the eluent is a mixed solvent of ethanol and dichloromethane, and the volume ratio of ethanol to dichloromethane is 1:11), and distill under reduced pressure to obtain intermediate 1; the amount of 2-amino-4,6-dichloro-1,3,5-triazine, diallylamine, triethylamine and DMSO is 13.2 g: 10.5 mL: 16.7 mL: 130 mL;
[0016] Triethylamine is used as an acid binding agent, and the molar ratio of 2-amino-4,6-dichloro-1,3,5-triazine and diallylamine is controlled to be 1:1.05-1.1. A -Cl of 2-amino-4,6-dichloro-1,3,5-triazine and -NH- of diallylamine undergo a nucleophilic substitution reaction. The reaction process is as follows:
[0017]
[0018] S2. Under nitrogen protection, dodecafluoroheptyl methacrylate, DBU (1,8-diazobisspiro[5.4.0]undec-7-ene) and DMSO were added to a three-necked flask, stirred evenly, and then the mixed solution of intermediate 1 and DMSO was slowly added. After the addition was completed, the temperature was raised to 60°C and the reaction was carried out for 48 hours. After the reaction was completed, it was distilled under reduced pressure, purified by column chromatography (the eluent was a mixed solvent of benzene and methanol, and the volume ratio of benzene and methanol was 19:1), and distilled under reduced pressure to obtain intermediate 2; the usage ratio of intermediate 1, dodecafluoroheptyl methacrylate, DBU and DMSO was 15.8 g:21 mL:1 mL:180 mL;
[0019] Under the catalytic action of DBU, the molar ratio of intermediate 1 to dodecafluoroheptyl methacrylate is controlled to be 1:1.1-1.2, and intermediate 1 and dodecafluoroheptyl methacrylate undergo Michael addition reaction. The reaction process is as follows:
[0020]
[0021] S3. Add intermediate 2, pyridine and DMF (N,N-dimethylformamide) to a dry three-necked flask under nitrogen protection, stir thoroughly until completely dissolved, then slowly add a mixed solution of flame retardant FRC-6 (N,N-bis(2-hydroxyethyl)aminomethylenephosphonic acid diethyl ester) and DMF, heat to 50°C, stir and react for 3 hours, cool to room temperature after the reaction, distill under reduced pressure, purify by column chromatography (the eluent is a mixed solvent of chloroform and ether, and the volume ratio of chloroform and ether is 9:1), and distill under reduced pressure to obtain an auxiliary agent. The dosage ratio of intermediate 2, flame retardant FRC-6, pyridine and DMF is 40.4g:7.66g:7.5mL:220mL.
[0022] Under heating conditions, pyridine is used as an acid-binding agent, and the molar ratio of intermediate 2 and flame retardant FRC-6 is controlled to be 2.2:1. Then, -Cl of intermediate 2 and -OH of flame retardant FRC-6 undergo substitution reaction. The reaction process is as follows:
[0023]
[0024] The auxiliary agent of the present invention contains rich phosphorus and nitrogen halogen-free flame retardant elements. Organic phosphorus decomposes to generate phosphorus oxygen-containing acids. The phosphorus oxygen-containing acids can promote the formation of a carbon layer on the substrate. A large amount of carbon layer plays a role in blocking the flow of combustible gas and heat, thereby achieving a flame retardant effect. Under the action of nitrogen element, the carbon layer formed on the surface of the substrate will expand and foam to form a porous foam structure. The expanded porous foam-like carbon layer will further block the process of heat and oxygen exchange between the substrate and the outside world, further improving the flame retardant effect. At the same time, a large amount of non-combustible gases such as H2O, NH3, CO2, NO2, etc. are released during the combustion process, which can dilute the concentration of combustible gas and delay the spread of flames.
[0025] The additives also contain abundant fluorine atoms. Since the covalent radius of fluorine atoms is slightly larger than that of hydrogen atoms, which is equivalent to half the length of CC bonds, fluorine atoms can shield the carbon chains well and maintain high stability. At the same time, since the polarizability of CF bonds is small and the bond distance is short, the intermolecular cohesion of compounds containing a large number of CF bonds is small, and the surface free energy is reduced, forming a unique property that can effectively prevent wetting and penetration of various liquids such as water-based stains and oily stains. These characteristics work together to make additives rich in fluorine atoms show good hydrophobicity and oleophobicity.
[0026] The additive contains abundant terminal carbon-carbon double bonds, which can react chemically with the carbon-carbon double bonds of the EPDM side chain under the action of the initiator, so that the additive is grafted on the EPDM side chain and stably exists in the cable material, and is not easy to migrate and escape. At the same time, the double bonds in the additive can also react chemically with the carbon-carbon double bonds on the surface of the modified silica under the action of the initiator, which makes the additive grafted on the surface of the modified silica, greatly reducing the surface energy of the modified silica, so that it can be highly dispersed in the cable material, giving full play to the wear resistance and insulation effects. Therefore, the additive, the modified silica and the EPDM form a hybrid cross-linked network structure, thereby making the flame retardant performance and hydrophobic and oleophobic performance of the cable material of the present invention more excellent and stable.
[0027] Furthermore, the antioxidant is a mixture of antioxidant D and antioxidant SP in a mass ratio of 1:3.
[0028] Furthermore, the antioxidant is one or more of antioxidant 565, antioxidant 1010, and antioxidant 168.
[0029] Furthermore, the ultraviolet absorber is one or more of ultraviolet absorber UV-O, ultraviolet absorber UV-531, ultraviolet absorber UVP-327, and light stabilizer 744.
[0030] Furthermore, the initiator is di-tert-butyl peroxide.
[0031] A method for preparing an oil-resistant power cable material for a petroleum drilling platform comprises the following steps:
[0032] The EPDM rubber, hydrogenated nitrile rubber and chloroprene rubber are mixed evenly, placed in a single-screw extruder for blending and granulation to obtain a mixed elastomer; the mixed elastomer and modified white carbon black, additives, antioxidants, antioxidants, ultraviolet absorbers and initiators are added to an internal mixer, mixed evenly and then kneaded, and after kneading, the mixture is put into a twin-screw extruder for extrusion to obtain a cable material.
[0033] The beneficial effects of the present invention are as follows: the additive contains abundant fluorine atoms and halogen-free flame retardant elements such as nitrogen and phosphorus, and the end of the additive contains a plurality of carbon-carbon double bonds, and the surface of the modified silica also has abundant double bonds. Therefore, under the action of the initiator, there is a chemical reaction between the additive, silica and EPDM rubber, and the three are cross-linked to form a hybrid cross-linked network structure. The additive and filler can not only be evenly dispersed in the cable material, but also can stably exist in the cable material, give full play to their own effects, and are not easy to migrate and fall out. Therefore, the cable material of the present invention also has excellent properties such as wear resistance, flame retardancy, hydrophobicity, oleophobicity and insulation for a long time. DETAILED DESCRIPTION
[0034] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] Example 1
[0036] Preparation of modified white carbon black, the specific steps are as follows:
[0037] Add 24g of white carbon black and 200mL of acetone into a 500mL three-necked flask, add 3g of maleic anhydride and 0.75g of DMAP while stirring, after adding, stir and heat to 50℃, keep warm for 12h, after the reaction is completed, filter, wash with deionized water 3 times, then wash with anhydrous ethanol 3 times, and dry at 80℃ for 12h to obtain modified white carbon black.
[0038] Example 2
[0039] Preparation of auxiliary agent, the specific steps are as follows:
[0040] S1. Under nitrogen protection, 13.2 g of 2-amino-4,6-dichloro-1,3,5-triazine, 16.7 mL of triethylamine and 130 mL of DMSO were added to a 250 mL dry brown three-necked flask, stirred until completely dissolved, and then 10.5 mL of diallylamine was slowly added. After the addition was completed, the temperature was controlled at 0-5°C to react for 8 hours. After the reaction was completed, it was distilled under reduced pressure, purified by column chromatography (the eluent was a mixed solvent of ethanol and dichloromethane, and the volume ratio of ethanol to dichloromethane was 1:11), and distilled under reduced pressure to obtain intermediate 1;
[0041] S2, under nitrogen protection, add 21 mL of dodecafluoroheptyl methacrylate, 1 mL of DBU and 140 mL of DMSO into a 500 mL three-necked flask, stir evenly, then slowly add a mixed solution of 15.8 g of intermediate 1 and 40 mL of DMSO, heat to 60 ° C after the addition is complete, react for 48 hours, and after the reaction is completed, distill under reduced pressure, purify by column chromatography (the eluent is a mixed solvent of benzene and methanol, and the volume ratio of benzene and methanol is 19:1), and distill under reduced pressure to obtain intermediate 2;
[0042] S3. Under nitrogen protection, add 40.4 g of intermediate 2, 7.5 mL of pyridine and 200 mL of DMF into a 500 mL dry three-necked flask, stir thoroughly until completely dissolved, then slowly add a mixed solution of 7.66 g of flame retardant FRC-6 and 20 mL of DMF, then heat to 50 ° C, stir and react for 3 hours, cool to room temperature after the reaction, distill under reduced pressure, purify by column chromatography (the eluent is a mixed solvent of chloroform and ether, and the volume ratio of chloroform and ether is 9:1), and distill under reduced pressure to obtain an auxiliary agent.
[0043] Example 3
[0044] The specific steps for preparing cable materials are as follows:
[0045] 70 parts of ethylene propylene diene monomer rubber, 20 parts of hydrogenated nitrile rubber and 8 parts of chloroprene rubber are mixed uniformly, and then placed in a single-screw extruder for blending and granulation to obtain a mixed elastomer; the mixed elastomer and 15 parts of the modified white carbon black prepared in Example 1, 10 parts of the auxiliary agent prepared in Example 2, 0.45 parts of antioxidant D, 1.35 parts of antioxidant SP, 0.8 parts of antioxidant 565, 0.8 parts of ultraviolet absorber UV-O and 0.5 parts of di-tert-butyl peroxide are added to an internal mixer, mixed uniformly and then kneaded, and then put into a twin-screw extruder for extrusion to obtain a cable material.
[0046] Example 4
[0047] The specific steps for preparing cable materials are as follows:
[0048] 75 parts of ethylene propylene diene monomer rubber, 26 parts of hydrogenated nitrile rubber and 10 parts of chloroprene rubber are mixed uniformly, placed in a single-screw extruder for blending and granulation to obtain a mixed elastomer; the mixed elastomer and 20 parts of the modified white carbon black prepared in Example 1, 12 parts of the auxiliary agent prepared in Example 2, 0.5 parts of antioxidant D, 1.5 parts of antioxidant SP, 1 part of antioxidant 1010, 1 part of ultraviolet absorber UV-531 and 0.8 parts of di-tert-butyl peroxide are added to an internal mixer, mixed uniformly and then kneaded, and then put into a twin-screw extruder for extrusion to obtain a cable material.
[0049] Example 5
[0050] The specific steps for preparing cable materials are as follows:
[0051] 80 parts of ethylene propylene diene monomer rubber, 30 parts of hydrogenated nitrile rubber and 12 parts of chloroprene rubber are mixed uniformly, placed in a single screw extruder for blending and granulation to obtain a mixed elastomer; the mixed elastomer and 25 parts of the modified white carbon black prepared in Example 1, 15 parts of the auxiliary agent prepared in Example 2, 0.6 parts of antioxidant D, 1.8 parts of antioxidant SP, 0.8 parts of antioxidant 1010, 0.4 parts of antioxidant 168, 0.8 parts of ultraviolet absorber UVP-327, 0.4 parts of light stabilizer 744 and 1 part of di-tert-butyl peroxide are added to an internal mixer, mixed uniformly and then kneaded, and then put into a twin-screw extruder for extrusion to obtain a cable material.
[0052] Comparative Example 1
[0053] The specific steps for preparing cable materials are as follows:
[0054] The remaining steps remain unchanged, only the modified silica in Example 5 is replaced by silica without any treatment, so as to prepare the cable material.
[0055] Comparative Example 2
[0056] The specific steps for preparing cable materials are as follows:
[0057] The remaining steps remain unchanged, only the auxiliary agent in Example 5 is replaced by 7.5 parts of 3-perfluorooctyl-1,2-propylene oxide and 7.5 parts of flame retardant FRC-2, thereby preparing a cable material.
[0058] Comparative Example 3
[0059] The remaining steps remain unchanged, only the modified silica in Example 5 is replaced by silica without any treatment, and the auxiliary agent is replaced by 7.5 parts of 3-perfluorooctyl-1,2-propylene oxide and 7.5 parts of flame retardant FRC-2, thereby preparing a cable material.
[0060] Performance Testing
[0061] The cable materials prepared in Examples 3-5 and Comparative Examples 1-3 were made into corresponding samples according to different standards, and the limiting oxygen index was tested by the method specified in GB / T 2406.2-2009; the vertical burning grade was tested by UL94; the wear rate was determined by using a universal friction and wear tester, and the test conditions were: the test force was 30N, the speed was 250r / min, and the test time was 30min. The wear rate was calculated by the formula: wear rate = (mass before wear - mass after wear) / mass before wear × 100%. The test results are shown in Table 1 below:
[0062] Table 1
[0063] Test items Limiting oxygen index % Vertical burning level Wear rate % Example 3 42.2 V-0 0.81 Example 4 42.7 V-0 0.75 Example 5 43.1 V-0 0.70 Comparative Example 1 40.1 V-0 5.12 Comparative Example 2 35.2 V-2 1.47 Comparative Example 3 34.6 V-2 5.19
[0064] It can be seen from the test results in Table 1 that the cable materials prepared in Examples 3-5 of the present invention have excellent flame retardancy and wear resistance.
[0065] The cable materials prepared in Examples 3-5 and Comparative Examples 1-3 were cut into 1 cm 3 The small cubes were immersed in distilled water at 10℃ and 35℃ and octane at 10℃ and 35℃ for 15 days respectively, and the changes in the morphology of the small cubes were observed. The test results are shown in Table 2 below:
[0066] Table 2
[0067]
[0068]
[0069] It can be seen from the test results in Table 2 that the cable materials prepared in Examples 3-5 of the present invention have excellent hydrophobic and oleophobic properties and can be used as power cable materials for oil-resistant oil drilling platforms.
[0070] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0071] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A power cable material for oil-resistant oil drilling platforms, characterized in that: The invention comprises the following raw materials in parts by weight: 70-80 parts of EPDM rubber, 20-30 parts of hydrogenated nitrile rubber, 8-12 parts of chloroprene rubber, 15-25 parts of modified white carbon black, 10-15 parts of auxiliary agent, 1.8-2.4 parts of antioxidant, 0.8-1.2 parts of antioxidant, 0.8-1.2 parts of ultraviolet absorber and 0.5-1 parts of initiator; Wherein, the modified silica is prepared by the following steps: Add white carbon black and acetone into a flask, stir, add maleic anhydride and DMAP, react at 50°C for 12h, filter, wash and dry to obtain modified white carbon black; The auxiliary agent is prepared by the following steps: S1. Add 2-amino-4,6-dichloro-1,3,5-triazine, triethylamine and DMSO into a flask under nitrogen protection, stir, add diallylamine, react at 0-5°C for 8h, distill under reduced pressure, purify by column chromatography, and distill under reduced pressure to obtain intermediate 1; S2, under nitrogen protection, dodecafluoroheptyl methacrylate, DBU and DMSO were added to a flask, stirred, and intermediate 1 and DMSO were added, reacted at 60° C. for 48 h, distilled under reduced pressure, purified by column chromatography, and distilled under reduced pressure to obtain intermediate 2; S3. Under nitrogen protection, add intermediate 2, pyridine and DMF into a flask, stir, add flame retardant FRC-6 and DMF, react at 50°C for 3h, distill under reduced pressure, purify by column chromatography, and distill under reduced pressure to obtain an auxiliary agent.
2. The oil-resistant power cable material for oil drilling platform according to claim 1, characterized in that: The mass ratio of white carbon black to maleic anhydride is 8:
1.
3. The oil-resistant power cable material for oil drilling platform according to claim 1, characterized in that: The amounts of 2-amino-4,6-dichloro-1,3,5-triazine, diallylamine, triethylamine and DMSO used in step S1 are 13.2 g: 10.5 mL: 16.7 mL: 130 mL.
4. The oil-resistant power cable material for oil drilling platform according to claim 1, characterized in that: The usage ratio of intermediate 1, dodecafluoroheptyl methacrylate, DBU and DMSO in step S2 is 15.8 g:21 mL:1 mL:180 mL.
5. The oil-resistant power cable material for oil drilling platform according to claim 1, characterized in that: The usage ratio of intermediate 2, flame retardant FRC-6, pyridine and DMF in step S3 is 40.4 g:7.66 g:7.5 mL:220 mL.
6. The oil-resistant power cable material for oil drilling platform according to claim 1, characterized in that: The antioxidant is a mixture of antioxidant D and antioxidant SP in a mass ratio of 1:
3.
7. The oil-resistant power cable material for oil drilling platform according to claim 1, characterized in that: The antioxidant is one or more of antioxidant 565, antioxidant 1010, and antioxidant 168.
8. The oil-resistant power cable material for oil drilling platform according to claim 1, characterized in that: The ultraviolet absorber is one or more of the ultraviolet absorber UV-O, ultraviolet absorber UV-531, ultraviolet absorber UVP-327, and light stabilizer 744.
9. The oil-resistant power cable material for oil drilling platform according to claim 1, characterized in that: The initiator is di-tert-butyl peroxide.
10. The method for preparing an oil-resistant power cable material for a petroleum drilling platform according to claim 1, characterized in that: The following steps are involved: The EPDM rubber, hydrogenated nitrile rubber and chloroprene rubber are mixed evenly, placed in a single-screw extruder for blending and granulation to obtain a mixed elastomer; the mixed elastomer and modified white carbon black, additives, antioxidants, antioxidants, ultraviolet absorbers and initiators are added to an internal mixer, mixed evenly and then kneaded, and after kneading, the mixture is put into a twin-screw extruder for extrusion to obtain a cable material.
Citation Information
Cited By
Low-smoke flame-retardant TPE composite material and preparation method thereof
CN119220043A