Modified polylactic acid sheet as well as preparation method and application thereof
Through the melt blending and unidirectional stretching of modified tackifying resin and polylactic acid, the brittleness problem of polylactic acid sheet after physical aging and heat treatment is solved, its toughness and aging resistance are improved, and food packaging and other high performance needs in the field.
Patent Information
- Application Number
- CN202310516171.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-09
- Publication Date
- 2024-11-12
AI Technical Summary
Existing polylactic acid sheets are prone to physical aging during the warehousing logistics process and become brittle, and the blister products after heat setting are prone to radical brittle during the warehousing logistics stage, which cannot meet the comprehensive performance requirements of high toughness and physical aging resistance.
Modified tackifying resin and polylactic acid are melt blended, and modified tackifying resin is prepared by graft modification and esterification reaction. Combined with unidirectional stretching treatment, it is prepared to prepare a modified polypeptide with high toughness and physical aging resistance. Lactic acid sheet.
The tensile strength, elongation of break and impact strength of the polylactic acid sheet are improved, and the storage stability is ensured below the glass transition temperature, avoiding the transition from toughness to brittleness, and meeting the application needs in the fields of food packaging and other fields.
Smart Images

Figure BDA0004219216510000111 
Figure HDA0004219216520000011
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of extruded sheets, and in particular relates to a modified polylactic acid sheet and a preparation method and application thereof (disposable dinner plates, packaging boxes, etc.). Background Art
[0002] Due to the booming takeout market, the demand for packaging materials such as takeaway boxes and disposable plates has increased dramatically. However, the raw materials of relevant packaging materials are basically derived from petrochemical resources, such as polyolefins, polyethylene terephthalate, etc. However, the precipitation of petroleum-based resins themselves and related additives poses uncertainty to food safety; in addition, the non-degradability of petroleum-based resins can easily cause serious "white" pollution to the environment, casting a shadow on the widespread application of petroleum-based sheets in the packaging field. Therefore, it is particularly necessary to develop biodegradable polymer sheets that can be used in the field of food packaging.
[0003] Among them, the more typical biodegradable polymer is polylactic acid (PLA). PLA has good biocompatibility and biodegradability. It can eventually form carbon dioxide and water after being decomposed by microorganisms during the composting process. It is one of the earliest biodegradable polymers certified by the US Food and Drug Administration (FDA). With the maturity of PLA large-scale production technology and the gradual reduction of its production cost, PLA has attracted widespread attention in the fields of biomedicine, packaging, textiles, etc. in recent years. However, polylactic acid has problems such as high brittleness and poor toughness; in particular, physical aging is very likely to occur below the glass transition temperature, making polylactic acid rapidly brittle (Macromolecules 2007, 40, 9664-9671; Macromolecules 2019, 52, 8878-8894; Polymer 2020, 186, 122014;
[0004] Macromolecules 2019, 52, 5429-5441).
[0005] There are many public reports on the preparation of PLA sheets, among which the main focus is on improving the toughness of the sheets. CN102250454A discloses a low-cost, fully degradable, highly flexible polylactic acid composite material and its preparation method. The weight proportions of each component in the composite material of 100 parts by weight are: 30-70 parts of PLA, 20-50 parts of calcium carbonate, 0-20 parts of plasticizer and 0.5-2 parts of functional additives. The obtained composite material not only has improved toughness, but also has a good feel and greatly reduced costs. CN103540111A discloses a high-strength, high-temperature resistant fully degradable polylactic acid sheet and its manufacturing method. The addition of elastomers and inorganic fillers simultaneously plays a synergistic role, improving strength while exerting the toughening effect of the elastomer. CN105602215A discloses a biodegradable heat-resistant sheet and a preparation method thereof. The weight proportions of the components in 100 parts of the sheet are: 20-50 parts of PLA, 35-55 parts of PBS, 0-10 parts of polyester, 1-25 parts of nucleating enhancer, 0.5-5 parts of auxiliary agent and 0-0.5 parts of UV inhibitor, which solves the current problems of high brittleness of polylactic acid sheets, high cost of calendered sheets, and narrow application range. CN114702799A discloses a biodegradable polylactic acid blister sheet, wherein the weight proportions of each component in the sheet of 100 parts by weight are: 50-95 parts of PLA, 3-35 parts of PBAT, 3-10 parts of compatibilizer, 2-20 parts of nucleating agent, 0.01-5 parts of dispersant, 0.01-5 parts of plasticizer, 0.01-5 parts of coupling agent, 0.01-5 parts of chain extender and 1-95 parts of filler, and the polylactic acid sheet with improved toughness is obtained by strictly controlling the content of each component. In addition, CN112521732A discloses a biaxially stretched polylactic acid film material resistant to physical aging, a preparation method thereof and an application thereof, wherein the polylactic acid melt is stretched and oriented, and then rapidly quenched to maintain the oriented structure and inhibit the relaxation of the molecular chain to achieve the effect of physical aging resistance.
[0006] Although the above-mentioned known technologies all prepare toughened and modified polylactic acid sheets, they still have the following limitations: (1) polylactic acid sheets are easily physically aged during the storage and logistics stage, causing them to become brittle; (2) polylactic acid sheets undergo preheating treatment before blistering, and the resulting blister products are easily physically aged during the storage and logistics stage, causing them to become brittle rapidly; (3) polylactic acid blister products that have been heat-set are easily physically aged during the storage and logistics stage, causing them to become brittle rapidly. Therefore, it is necessary to develop new polylactic acid sheets with high toughness and resistance to physical aging and their preparation methods to meet the high requirements for comprehensive performance put forward by various applications. Summary of the invention
[0007] The first purpose of the present invention is to overcome the problems of insufficient toughness and poor physical aging resistance of polylactic acid sheets in the prior art, and to provide a modified polylactic acid sheet and its preparation method and application, wherein the toughness and physical aging resistance of the modified polylactic acid sheet can be improved.
[0008] A modified polylactic acid sheet is a melt blend, wherein the weight parts of each raw material in 100 weight parts of the sheet are: 65-99 parts of polylactic acid, 1-35 parts of modified tackifying resin; the modified tackifying resin is prepared by the following method: the tackifying resin is mixed with maleic anhydride for grafting modification, and then esterified with lactic acid oligomer to obtain the modified tackifying resin.
[0009] Preferably, the weight proportions of each component in 100 parts of the sheet are: 75-95 parts of polylactic acid, 5-25 parts of modified tackifying resin. More preferably, the weight proportions of each component in 100 parts of the sheet are: 82-90 parts of polylactic acid, 10-18 parts of modified tackifying resin.
[0010] Preferably, the weight average molecular weight of the polylactic acid is 80,000-500,000, and the molar content of the L optical isomer in the polylactic acid is 85-99%; more preferably, the weight average molecular weight of the polylactic acid is 150,000-350,000, and the molar content of the L optical isomer in the polylactic acid is 92-98%;
[0011] Preferably, the weight average molecular weight of the modified tackifying resin is 300-8000, and the molar grafting ratio is 15-80%. More preferably, the weight average molecular weight of the modified tackifying resin is 800-3000, and the molar grafting ratio is 30-55%.
[0012] Specifically, the preparation method of the modified tackifying resin comprises the following steps:
[0013] Step (1), melt blending 80-98 parts by weight of a tackifying resin (Cx), 2-20 parts by weight of maleic anhydride (MAH), and 0.1-1.2 parts by weight of dicumyl peroxide to form a maleic anhydride grafted tackifying resin (Cx-g-MAH), the reaction temperature being 100-150° C., and the reaction time being 4-12 minutes;
[0014] Step (2), mixing 40-60 parts by weight of L-lactic acid, 40-60 parts by weight of 1,4-butanediol and 0.1-1.2 parts by weight of stannous chloride for esterification reaction to form lactic acid oligomers, the reaction temperature is 110-155° C., the reaction pressure is 0.5-101 kPa, and the reaction time is 4-12 hours;
[0015] Step (3), further mixing 35-65 parts by weight of the maleic anhydride grafted tackifying resin (Cx-g-MAH) obtained in step (1) with 35-65 parts by weight of the lactic acid oligomer obtained in step (2) and 0.1-1.2 parts by weight of stannous octoate to carry out an esterification reaction to obtain the modified tackifying resin, the reaction temperature is 155-195° C., the reaction pressure is 0.5-101 kPa, and the reaction time is 1-4 hours.
[0016] Preferably, the lactic acid oligomer is a hydroxy-terminated lactic acid oligomer, and the molecular weight of the lactic acid oligomer is 72-720.
[0017] Preferably, the tackifying resin includes one or more combinations of C5 tackifying resin, C5 hydrogenated tackifying resin, C9 hydrogenated tackifying resin, C9 cold-polymerized tackifying resin, C9 hot-polymerized tackifying resin, C5 / C9 copolymerized tackifying resin, terpene resin, and rosin ester, but is not limited thereto.
[0018] According to the present invention, the modified polylactic acid sheet prepared by the method of the present invention has a tensile strength of 54-83 MPa, an elongation at break of 126%-243%, and a notched impact strength of 6.5-17.4 KJ / m 2 , the glass transition temperature of polylactic acid is 46-65°C. g After sufficient storage (shelf life), the change rate of tensile strength before and after storage is generally less than 15%; the change rate of impact strength before and after storage is also less than 15%; the change rate of elongation at break is generally less than 35%, and there is no transition from toughness to brittleness; wherein, the storage time is not limited; however, generally speaking, the time is ≥5 hours.
[0019] The second object of the present invention is to provide a method for preparing a modified polylactic acid sheet, the method comprising: blending polylactic acid and a modified tackifying resin, melt extruding, casting, and uniaxially stretching to obtain a modified polylactic acid sheet.
[0020] Preferably, the extrusion temperature of the melt extrusion is 160-220°C, and the casting roll temperature of the cast sheet is 20-50°C; more preferably, the extrusion temperature is 180-210°C, and the casting roll temperature is 20-40°C.
[0021] Preferably, the stretching temperature of the uniaxial stretching is 75-145° C., and the stretching ratio is 2-8 times; more preferably, the stretching temperature is 90-130° C., and the stretching ratio is 3-7 times.
[0022] Preferably, the composition further comprises drying before melt extrusion.
[0023] Preferably, the drying temperature is 90-98° C. and the drying time is 5-10 h.
[0024] The third object of the present invention is to provide the use of the modified polylactic acid sheet as described above as a food packaging material.
[0025] The advantages of the technical solution provided by the present invention are at least:
[0026] (1) The present invention improves the stretchability of the polylactic acid sheet by combining polylactic acid with a specific component content with a modified tackifying resin, thereby obtaining a modified polylactic acid sheet with improved toughness and physical aging resistance;
[0027] (2) The conventional sheet extrusion equipment and conventional process of the present invention can give the modified polylactic acid sheet the property of physical aging resistance, without the need for specially customized high-multiple drafting and quenching equipment;
[0028] (3) The modified polylactic acid sheet prepared by the present invention is further heat-treated and the obtained blister products also have the property of physical aging resistance, thus solving the technical problem that the polylactic acid sheet resistant to physical aging cannot be heat-treated;
[0029] (4) The present invention uses a relatively high molecular weight polylactic acid, which can improve the melt strength of the blending system and improve the mechanical properties of the polylactic acid sheet; the polylactic acid selected has a relatively high molar content of L optical isomers, which can improve the crystallization ability of the blending system, thereby improving the crystallinity and mechanical properties of the modified polylactic acid sheet; the modified tackifying resin with a medium weight average molecular weight and molar grafting ratio is selected, which significantly improves the compatibility of the tackifying resin with polylactic acid, can improve the melt strength of the blending system and the toughness of the modified polylactic acid sheet, and endows the modified polylactic acid sheet with physical aging resistance; wherein the modified tackifying resin forms a viscoelastic three-dimensional network structure in the polylactic acid matrix, reduces the yield stress during the tensile deformation process, and enables the modified polylactic acid sheet to maintain tough fracture without the transition from toughness to brittleness, thereby endowing the modified polylactic acid sheet with the property of physical aging resistance, breaking through the performance bottleneck of conventional polylactic acid sheets that are prone to physical aging and become brittle, thereby fully meeting the use requirements and greatly expanding its application field. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 3 is the stress-strain curve of the modified polylactic acid sheet prepared in Example 1 of the present invention before and after physical aging. DETAILED DESCRIPTION
[0031] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0032] In the present invention, unless otherwise specified, "PLA" refers to polylactic acid; and "LA" refers to lactic acid.
[0033] The first aspect of the present invention provides a modified polylactic acid sheet, which is a melt blend, wherein the weight parts of each raw material in 100 parts of the sheet are: 65-99 parts of polylactic acid, 1-35 parts of modified tackifying resin; the modified tackifying resin is prepared by the following method: the tackifying resin is mixed with maleic anhydride for grafting modification, and then esterified with lactic acid oligomers to obtain the modified tackifying resin;
[0034] Specifically, the modified tackifying resin is prepared by the following method:
[0035] Step (1), melt blending 80-98 parts by weight of tackifying resin Cx, 2-20 parts by weight of maleic anhydride MAH, and 0.1-1.2 parts by weight of dicumyl peroxide to form a maleic anhydride grafted tackifying resin Cx-g-MAH, the reaction temperature is 100-150° C., and the reaction time is 4-12 minutes;
[0036] Step (2), mixing 40-60 parts by weight of L-lactic acid, 40-60 parts by weight of 1,4-butanediol and 0.1-1.2 parts by weight of stannous chloride for esterification reaction to form lactic acid oligomers, the reaction temperature is 110-155° C., the reaction pressure is 0.5-101 kPa, and the reaction time is 4-12 hours;
[0037] Step (3), further mixing 35-65 parts by weight of the maleic anhydride grafted tackifying resin Cx-g-MAH obtained in step (1) with 35-65 parts by weight of the lactic acid oligomer obtained in step (2) and 0.1-1.2 parts by weight of stannous octoate to carry out esterification reaction to obtain the modified tackifying resin, the reaction temperature is 155-195°C, the reaction pressure is 0.5-101 kPa, and the reaction time is 1-4 hours.
[0038] The weight average molecular weight of the modified tackifying resin is 300-8000, and the molar grafting ratio is 15-80%; the molecular weight of the lactic acid oligomer is 72-720; and the lactic acid oligomer is a terminal hydroxyl lactic acid oligomer.
[0039] The weight average molecular weight of the polylactic acid is 80,000-500,000, and the molar content of the L optical isomer in the polylactic acid is 85-99%.
[0040] The second aspect of the present invention provides a method for preparing a modified polylactic acid sheet, the method comprising: blending polylactic acid and a modified tackifying resin, and then melt-extruding, casting, and uniaxially stretching to obtain a modified polylactic acid sheet.
[0041] The extrusion temperature of the melt extrusion is 160-220°C, and the casting roll temperature of the cast sheet is 20-50°C; the stretching temperature of the uniaxial stretching is 75-145°C, and the stretching ratio is 2-8 times;
[0042] The composition is further dried before being melt-extruded; the drying temperature is 90-98° C. and the drying time is 5-10 hours.
[0043] The third aspect of the present invention provides the use of the modified polylactic acid sheet as a food packaging material.
[0044] The present invention will be described in detail below by way of examples. In the following examples and comparative examples:
[0045] (1) Glass transition temperature was measured by differential scanning calorimetry (DSC);
[0046] (2) Mechanical properties (including tensile strength and elongation at break) were measured using a universal tensile testing machine (refer to national standard GB / T14344);
[0047] (3) Impact properties (such as notched impact strength) are measured by an Izod impact tester (refer to national standard GB / T1843-2008);
[0048] (4) Polylactic acid, tackifying resin, lactic acid and maleic anhydride were all purchased from commercial sources.
[0049] The preparation method of the modified tackifying resin used in the following examples includes:
[0050] 1) 85 parts by weight of a tackifying resin (one of a C5 tackifying resin, a terpene resin, and a rosin ester) are melt-blended with 15 parts by weight of maleic anhydride (MAH) and 0.6 parts by weight of dicumyl peroxide to form a tackifying resin having a carboxylic acid group by grafting, the reaction temperature being 120° C. and the reaction time being 10 min;
[0051] (2) 50 parts by weight of L-lactic acid, 50 parts by weight of 1,4-butanediol and 0.8 parts by weight of stannous chloride were mixed for esterification reaction to form terminal hydroxyl lactic acid oligomers, the reaction temperature was 130° C., the reaction pressure was 2 kPa, and the reaction time was 6 h;
[0052] (3) 58 parts by weight of the maleic anhydride grafted tackifier resin was further mixed with 42 parts by weight of terminal hydroxyl lactic acid oligomer and 0.4 parts by weight of stannous octoate for esterification reaction to form a lactic acid oligomer modified tackifier resin. The reaction temperature was 160° C., the reaction pressure was 10 kPa, and the reaction time was 2 h to obtain a modified tackifier resin.
[0053] Example 1
[0054] This embodiment is intended to illustrate the modified polylactic acid sheet prepared by the composition and method of the present invention.
[0055] (1) Take polylactic acid with a weight average molecular weight of 200,000, and a molar content of L optical isomer in PLA of 98%; a modified tackifying resin with a weight average molecular weight of 1200, and a molar grafting ratio of 42%; wherein the weight parts of each component in 100 parts by weight of the blend are: 90 parts of polylactic acid and 10 parts of the modified tackifying resin; the blend obtained by melt extrusion of the composition is hot-air dried at a drying temperature of 95±2° C. for 8 hours, and the water content is 42 ppm;
[0056] (2) The dried blend was melt-extruded and cast through a conventional sheet extrusion device, the melt extrusion temperature was 185°C, and the casting roller temperature was 35°C; then, the modified polylactic acid sheet was obtained by uniaxial stretching, cooling and winding, the stretching temperature was 95°C, and the stretching ratio was 4 times. The properties of the modified polylactic acid sheet were tested, and the test results are shown in Table 1. The stress-strain curves before and after physical aging are shown in Table 1. Figure 1 shown.
[0057] Example 2
[0058] This embodiment is intended to illustrate the modified polylactic acid sheet prepared by the composition and method of the present invention.
[0059] (1) Take polylactic acid with a weight average molecular weight of 250,000 and a molar content of L optical isomer in PLA of 97%; a modified tackifying resin with a weight average molecular weight of 2000 and a molar grafting ratio of 48%; wherein the weight parts of each component in 100 parts by weight of the blend are: 82 parts of polylactic acid and 18 parts of the modified tackifying resin; the blend obtained by melt extrusion of the composition is hot-air dried at a drying temperature of 94±2° C. for 7 hours, and the water content is 48 ppm;
[0060] (2) The dried blend was melt-extruded and cast through a conventional sheet extrusion device, the melt extrusion temperature was 200°C, and the casting roll temperature was 25°C; then, the modified polylactic acid sheet was obtained by uniaxial stretching, cooling and winding, the stretching temperature was 115°C, and the stretching ratio was 6 times. The properties of the modified polylactic acid sheet were tested, and the test results are shown in Table 1.
[0061] Example 3
[0062] This embodiment is intended to illustrate the modified polylactic acid sheet prepared by the composition and method of the present invention.
[0063] (1) Take polylactic acid with a weight average molecular weight of 230,000 and a molar content of L optical isomer in PLA of 98%; a modified tackifying resin with a weight average molecular weight of 1700 and a molar grafting ratio of 45%; wherein the weight parts of each component in 100 parts by weight of the blend are: 86 parts of polylactic acid and 14 parts of the modified tackifying resin; the blend obtained by melt extrusion of the composition is hot-air dried at a drying temperature of 97±2°C for 8 hours, and the water content is 46ppm;
[0064] (2) The dried blend was melt-extruded and cast through a conventional sheet extrusion device, the melt extrusion temperature was 192°C, and the casting roll temperature was 28°C; then, the modified polylactic acid sheet was obtained by uniaxial stretching, cooling and winding, the stretching temperature was 102°C, and the stretching ratio was 5 times. The properties of the modified polylactic acid sheet were tested, and the test results are shown in Table 1.
[0065] Example 4
[0066] This embodiment is intended to illustrate the modified polylactic acid sheet prepared by the composition and method of the present invention.
[0067] (1) Take polylactic acid with a weight average molecular weight of 250,000, and a molar content of L optical isomer in PLA of 99%; a modified tackifying resin with a weight average molecular weight of 300, and a molar grafting ratio of 15%; wherein the weight parts of each component in 100 parts by weight of the blend are: 65 parts of polylactic acid and 35 parts of the modified tackifying resin; the blend obtained by melt extrusion of the composition is hot-air dried at a drying temperature of 98±2°C for 10 hours, and the water content is 38 ppm;
[0068] (2) The dried blend was melt-extruded and cast through a conventional sheet extrusion device, the melt extrusion temperature was 160°C, and the casting roll temperature was 50°C; then, the modified polylactic acid sheet was obtained by uniaxial stretching, cooling and winding, the stretching temperature was 75°C, and the stretching ratio was 5 times. The properties of the modified polylactic acid sheet were tested, and the test results are shown in Table 1.
[0069] Example 5
[0070] This embodiment is intended to illustrate the modified polylactic acid sheet prepared by the composition and method of the present invention.
[0071] (1) Take polylactic acid with a weight average molecular weight of 250,000, and a molar content of L optical isomer in PLA of 95%; a modified tackifying resin with a weight average molecular weight of 8,000, and a molar grafting ratio of 80%; wherein the weight parts of each component in 100 parts by weight of the blend are: 80 parts of polylactic acid and 20 parts of the modified tackifying resin; the blend obtained by melt extrusion of the composition is hot-air dried at a drying temperature of 96±2° C. for 8 hours, and the water content is 52 ppm;
[0072] (2) The dried blend was melt-extruded and cast through a conventional sheet extrusion device, the melt extrusion temperature was 182°C, and the casting roll temperature was 40°C; then, the modified polylactic acid sheet was obtained by uniaxial stretching, cooling and winding, the stretching temperature was 95°C, and the stretching ratio was 8 times. The properties of the modified polylactic acid sheet were tested, and the test results are shown in Table 1.
[0073] Example 6
[0074] This embodiment is intended to illustrate the modified polylactic acid sheet prepared by the composition and method of the present invention.
[0075] (1) Take polylactic acid with a weight average molecular weight of 80,000, and a molar content of L optical isomer in PLA of 99%; a modified tackifying resin with a weight average molecular weight of 800, and a molar grafting ratio of 35%; wherein the weight parts of each component in 100 parts by weight of the blend are: 95 parts of polylactic acid and 5 parts of the modified tackifying resin; the blend obtained by melt extrusion of the composition is hot-air dried at a drying temperature of 94±2°C for 6 hours, and the water content is 54 ppm;
[0076] (2) The dried blend was melt-extruded and cast through a conventional sheet extrusion device, the melt extrusion temperature was 202°C, and the casting roll temperature was 35°C; then, the modified polylactic acid sheet was obtained by uniaxial stretching, cooling and winding, the stretching temperature was 120°C, and the stretching ratio was 3 times. The properties of the modified polylactic acid sheet were tested, and the test results are shown in Table 1.
[0077] Example 7
[0078] This embodiment is intended to illustrate the modified polylactic acid sheet prepared by the composition and method of the present invention.
[0079] (1) Take polylactic acid with a weight average molecular weight of 80,000, and a molar content of L optical isomer in PLA of 99%; a modified tackifying resin with a weight average molecular weight of 3,000, and a molar grafting ratio of 65%; wherein the weight parts of each component in 100 parts by weight of the blend are: 99 parts of polylactic acid and 1 part of the modified tackifying resin; the blend obtained by melt extrusion of the composition is hot-air dried at a drying temperature of 98±2°C for 5 hours, and the water content is 47ppm;
[0080] (2) The dried blend was melt-extruded and cast through a conventional sheet extrusion device, the melt extrusion temperature was 205°C, and the casting roll temperature was 32°C; then, the modified polylactic acid sheet was obtained by uniaxial stretching, cooling and winding, the stretching temperature was 130°C, and the stretching ratio was 2 times. The properties of the modified polylactic acid sheet were tested, and the test results are shown in Table 1.
[0081] Example 8
[0082] This embodiment is intended to illustrate the modified polylactic acid sheet prepared by the composition and method of the present invention.
[0083] (1) Take polylactic acid with a weight average molecular weight of 500,000, and a molar content of L optical isomer in PLA of 85%; a modified tackifying resin with a weight average molecular weight of 2000, and a molar grafting ratio of 40%; wherein the weight parts of each component in 100 parts by weight of the blend are: 96 parts of polylactic acid, 4 parts of the modified tackifying resin; the blend obtained by melt extrusion of the composition is hot-air dried at a drying temperature of 90±2° C., a drying time of 7 hours, and a water content of 64 ppm;
[0084] (2) The dried blend was melt-extruded and cast through a conventional sheet extrusion device, the melt extrusion temperature was 220°C, and the casting roll temperature was 20°C; then, the modified polylactic acid sheet was obtained by uniaxial stretching, cooling and winding, the stretching temperature was 145°C, and the stretching ratio was 4 times. The properties of the modified polylactic acid sheet were tested, and the test results are shown in Table 1.
[0085] Example 9
[0086] This embodiment is intended to illustrate the modified polylactic acid sheet prepared by the composition and method of the present invention.
[0087] (1) Take polylactic acid with a weight average molecular weight of 500,000 and a molar content of L optical isomer in PLA of 90%; a modified tackifying resin with a weight average molecular weight of 5,000 and a molar grafting ratio of 65%; wherein the weight parts of each component in 100 parts by weight of the blend are: 80 parts of polylactic acid and 20 parts of the modified tackifying resin; the blend obtained by melt extrusion of the composition is hot-air dried at a drying temperature of 92±2° C. for 10 hours, and the water content is 58 ppm;
[0088] (2) The dried blend was melt-extruded and cast through a conventional sheet extrusion device, the melt extrusion temperature was 200°C, and the casting roll temperature was 30°C; then, the modified polylactic acid sheet was obtained by uniaxial stretching, cooling and winding, the stretching temperature was 120°C, and the stretching ratio was 4 times. The properties of the modified polylactic acid sheet were tested, and the test results are shown in Table 1.
[0089] Example 10
[0090] This embodiment is intended to illustrate the modified polylactic acid sheet prepared by the composition and method of the present invention.
[0091] (1) Take polylactic acid with a weight average molecular weight of 80,000, and a molar content of L optical isomer in PLA of 95%; a modified tackifying resin with a weight average molecular weight of 300, and a molar grafting ratio of 28%; wherein the weight parts of each component in 100 parts by weight of the blend are: 85 parts of polylactic acid, 15 parts of the modified tackifying resin; the blend obtained by melt extrusion of the composition is hot-air dried at a drying temperature of 97±2°C for 8 hours, and the water content is 41ppm;
[0092] (2) The dried blend was melt-extruded and cast through a conventional sheet extrusion device, the melt extrusion temperature was 170°C, and the casting roll temperature was 45°C; then, the modified polylactic acid sheet was obtained by uniaxial stretching, cooling and winding, the stretching temperature was 90°C, and the stretching ratio was 6 times. The properties of the modified polylactic acid sheet were tested, and the test results are shown in Table 1.
[0093] Embodiment 11
[0094] This embodiment is intended to illustrate the modified polylactic acid sheet prepared by the composition and method of the present invention.
[0095] (1) Take polylactic acid with a weight average molecular weight of 500,000 and a molar content of L optical isomer in PLA of 94%; a modified tackifying resin with a weight average molecular weight of 8,000 and a molar grafting ratio of 75%; wherein the weight parts of each component in 100 parts by weight of the blend are: 82 parts of polylactic acid and 18 parts of the modified tackifying resin; the blend obtained by melt extrusion of the composition is hot-air dried at a drying temperature of 93±2° C. for 10 hours, and the water content is 39 ppm;
[0096] (2) The dried blend was melt-extruded and cast through a conventional sheet extrusion device, the melt extrusion temperature was 210°C, and the casting roll temperature was 25°C; then, the modified polylactic acid sheet was obtained by uniaxial stretching, cooling and winding, the stretching temperature was 125°C, and the stretching ratio was 5 times. The properties of the modified polylactic acid sheet were tested, and the test results are shown in Table 1.
[0097] Example 12
[0098] This embodiment is intended to illustrate the modified polylactic acid sheet prepared by the composition and method of the present invention.
[0099] (1) Take polylactic acid with a weight average molecular weight of 80,000, and a molar content of L optical isomer in PLA of 98%; a modified tackifying resin with a weight average molecular weight of 8,000, and a molar grafting ratio of 75%; wherein the weight parts of each component in 100 parts by weight of the blend are: 92 parts of polylactic acid, 8 parts of the modified tackifying resin; the blend obtained by melt extrusion of the composition is hot-air dried at a drying temperature of 97±2°C for 9 hours, and the water content is 39 ppm;
[0100] (2) The dried blend was melt-extruded and cast through a conventional sheet extrusion device, the melt extrusion temperature was 180°C, and the casting roll temperature was 35°C; then, the modified polylactic acid sheet was obtained by uniaxial stretching, cooling and winding, the stretching temperature was 95°C, and the stretching ratio was 6 times. The properties of the modified polylactic acid sheet were tested, and the test results are shown in Table 1.
[0101] Embodiment 13
[0102] This embodiment is intended to illustrate the modified polylactic acid sheet prepared by the composition and method of the present invention.
[0103] (1) Take polylactic acid with a weight average molecular weight of 500,000 and a molar content of L optical isomer in PLA of 88%; a modified tackifying resin with a weight average molecular weight of 300 and a molar grafting ratio of 32%; wherein the weight parts of each component in 100 parts by weight of the blend are: 70 parts of polylactic acid and 30 parts of the modified tackifying resin; the blend obtained by melt extrusion of the composition is hot-air dried at a drying temperature of 93±2° C. for 6 hours, and the water content is 45 ppm;
[0104] (2) The dried blend was melt-extruded and cast into sheets through conventional sheet extrusion equipment, with the melt extrusion temperature being 190°C and the casting roll temperature being 30°C; subsequently, the modified polylactic acid sheet was obtained by uniaxial stretching, cooling and winding, with the stretching temperature being 115°C and the stretching ratio being 7 times. The properties of the modified polylactic acid sheet were tested, and the test results are shown in Table 1.
[0105] Comparative Example 1
[0106] The method of Example 2 was followed, except that "18 parts of modified tackifying resin" was replaced by "50 parts". The test results are shown in Table 1.
[0107] Comparative Example 2
[0108] The method of Example 2 was followed, except that no modified tackifying resin was added. The test results are shown in Table 1.
[0109] Comparative Example 3
[0110] The method of Example 7 was followed, except that no modified tackifying resin was added. The test results are shown in Table 1.
[0111] Table 1 Performance test results of products of Examples 1-13 and Comparative Examples 1-3
[0112]
[0113] As can be seen from Table 1, the modified polylactic acid sheet of the present invention has good comprehensive performance, breaking through the performance bottleneck of conventional polylactic acid sheets that are prone to physical aging and become brittle, thereby fully meeting the use requirements and being applicable to the fields of food packaging materials.
[0114] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A modified polylactic acid sheet, which is a melt blend, characterized in that: 100 parts by weight of the sheet material comprises the following raw material components: 65-99 parts by weight of polylactic acid, 1-35 parts by weight of modified tackifying resin; The modified tackifying resin is prepared by the following method: 80-98 parts by weight of tackifying resin and 2-20 parts by weight of maleic anhydride are mixed for grafting modification to obtain maleic anhydride grafted tackifying resin; 35-65 parts by weight of maleic anhydride grafted tackifying resin and 35-65 parts by weight of lactic acid oligomer are esterified to obtain modified tackifying resin.
2. The modified polylactic acid sheet according to claim 1, characterized in that: The lactic acid oligomer is a hydroxyl-terminated lactic acid oligomer.
3. The modified polylactic acid sheet according to claim 2, characterized in that: The lactic acid oligomer is prepared by the following method: 40-60 parts by weight of L-lactic acid, 40-60 parts by weight of 1,4-butanediol, and 0.1-1.2 parts by weight of stannous chloride are subjected to esterification reaction to form lactic acid oligomers.
4. The modified polylactic acid sheet according to claim 1, characterized in that: The tackifying resin Cx includes one or more of C5 tackifying resin, C5 hydrogenated tackifying resin, C9 hydrogenated tackifying resin, C9 cold-polymerized tackifying resin, C9 hot-polymerized tackifying resin, C5 / C9 copolymerized tackifying resin, terpene resin, and rosin ester.
5. The modified polylactic acid sheet according to any one of claims 1 to 4, characterized in that: The preparation method of the modified tackifying resin specifically comprises the following steps: Step (1), melt-blending the tackifying resin Cx, maleic anhydride MAH and dicumyl peroxide at 100-150° C. for 4-12 minutes to graft to form a maleic anhydride grafted tackifying resin Cx-g-MAH; Step (2), mixing L-lactic acid with 1,4-butanediol and stannous chloride, and subjecting the mixture to an esterification reaction at 110-155° C. and 0.5-101 kPa for 4-12 hours to form lactic acid oligomers; Step (3), mixing the maleic anhydride grafted tackifying resin Cx-g-MAH obtained in step (1) with the lactic acid oligomer and stannous octoate obtained in step (2), and subjecting the mixture to an esterification reaction at 155-195° C. and 0.5-101 kPa for 1-4 hours to obtain the modified tackifying resin.
6. The modified polylactic acid sheet according to claim 1, characterized in that: The weight average molecular weight of the polylactic acid is 80,000-500,000, and the molar content of the L optical isomer in the polylactic acid is 85-99%.
7. The modified polylactic acid sheet according to claim 1 or 6, characterized in that: The weight average molecular weight of the modified tackifying resin is 300-8000, and the molar grafting ratio is 15-80%.
8. A method for preparing the modified polylactic acid sheet according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: blending polylactic acid and modified tackifying resin, then melt-extruding, casting and uniaxially stretching to obtain a modified polylactic acid sheet.
9. The method according to claim 8, characterized in that The extrusion temperature of the melt extrusion is 160-220° C., the casting roll temperature of the cast sheet is 20-50° C., the stretching temperature of the uniaxial stretching is 75-145° C., and the stretching ratio is 2-8 times.
10. Use of the modified polylactic acid sheet according to any one of claims 1 to 7 as a disposable packaging material.
Citation Information
Cited By
Modified polylactic acid fiber as well as preparation method and application thereof
CN119571498A
Quaternary ammonium salt-oligomeric lactic acid double-graft polymerized rosin / polylactic acid antibacterial fiber and preparation method thereof
CN120554802A