High-performance polyurethane coating as well as preparation method and application thereof
By using polyurethane coating preparation method with components such as hexamethylene diisocyanate and polycarbonate diol, combined with rapid low-temperature evaporation and alternating stirring, the problem of pinhole and bubble defects during the paint drying process is solved, and high performance is achieved The structural strength and appearance of the coating.
Patent Information
- Application Number
- CN202411093310.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing polyurethane coatings are prone to form pinholes or bubble defects during drying, which affects the performance and appearance of the coating film. The reaction of isocyanate with water to form unstable carbamic acid, resulting in poor emulsification effect.
Using components such as hexamethylene diisocyanate, polycarbonate diol, acetone aqueous solution and coupling agent, the acetone evaporation is rapidly low-temperature and evaporation of water under reduced pressure, combined with alternating stirring, aliphatic long chain structure is formed that is easier to form agglomerate. , blocks the contact between isocyanate and water, prevents the formation of carbon dioxide, and achieves uniform coating through gas-assisted spraying technology.
Effectively prevent pinholes or bubble defects from forming inside the paint after film formation, improve structural strength and appearance effect, and ensure uniformity and high performance of the coating.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings, in particular to a high-performance polyurethane coating and a preparation method and application thereof. Background Art
[0002] CN112646475B discloses a method for preparing and applying a flame-retardant, wear-resistant, low-VOC polyurethane coating. The isocyanate in the invention is any one of 4,4-diphenylmethane diisocyanate, isophorone diisocyanate and toluene diisocyanate. 4,4-diphenylmethane diisocyanate has two aromatic rings, and toluene diisocyanate has one aromatic ring. They are more rigid, and the hard segments they form are more concentrated. At the same time, the hydrogen bonds are also more concentrated. The strong hydrogen bond force makes it difficult for the chain segments to move. During emulsification and dispersion, stronger shear force is required to disperse them. Strong shear force will destroy the hydration layer of the emulsion particles, resulting in fewer hydrophilic groups, thinner hydration layers, and easy aggregation to form larger particles. Isophorone diisocyanate is an alicyclic diisocyanate. Compared with 4,4-diphenylmethane diisocyanate and toluene diisocyanate, it has less rigidity and a relatively soft molecular chain. It is easy to disperse during emulsification, and the average particle size of the prepared waterborne polyurethane emulsion is relatively small. However, the two isocyanate groups in the isophorone diisocyanate molecule have an interconvertible nature, which causes the product of its reaction with polyols to be isomerized.
[0003] CN118085716B discloses a polyurethane coating for rubber and plastic thermal insulation materials and a preparation method thereof. The polyurethane coating in the invention is a water-based two-component polyurethane coating. Since the water-based two-component polyurethane coating uses water as a dispersion medium, isocyanate will inevitably react with water to generate unstable carbamic acid, which decomposes into amines and releases CO2. When the coating surface dries too quickly (caused by low humidity and high temperature), a large amount of carbon dioxide will stay in the film or form defects on the surface, forming a large number of pinholes or bubbles, which directly affect the final performance and appearance of the coating. In addition, if the isocyanate group is excessive, the generated amine will react with the isocyanate to generate urea, forming white floccules, which affects the distribution of polyurethane during the emulsification process, and then affects the emulsification effect and the quality of the final product. Summary of the invention
[0004] The purpose of the present invention is to provide a high-performance polyurethane coating and a preparation method and application thereof, so as to solve the problems raised in the above background technology.
[0005] To achieve the above object, on the one hand, the present invention provides the following technical scheme: a high-performance polyurethane coating, the high-performance polyurethane coating comprising the following components in parts by weight: 25-30 parts of hexamethylene diisocyanate, 45-60 parts of polycarbonate diol, 2-4 parts of dimethylol propionic acid, 4-8 parts of triethylamine, 2-5 parts of ethylenediamine, 0.2-0.4 parts of coupling agent KH-550, 8-12 parts of acetone aqueous solution, 2-4 parts of acetone, and 18-24 parts of deionized water;
[0006] The volume ratio of acetone to water in the acetone aqueous solution is (2-4):1;
[0007] The preparation method of the high-performance polyurethane coating comprises the following steps:
[0008] S1. Add hexamethylene diisocyanate and polycarbonate diol into a sample preparation tank, stir at 85° C. with a disperser at 800-1200 r / min for 20-30 min, and add acetone aqueous solution during stirring to obtain a prepolymer, the viscosity of the prepolymer is 1900-2000 cps;
[0009] S2. Cool the prepolymer to room temperature and place it in a vacuum tank. First, reduce the air pressure in the vacuum tank to 37-47 kPa by a vacuum pump and maintain it for 10 minutes. Then, reduce the air pressure in the vacuum tank to 61-71 kPa by a vacuum pump. Stir clockwise and counterclockwise alternately every 1 minute for 30 minutes. Finally, turn off the vacuum pump and take out the prepolymer.
[0010] S3, heating the prepolymer to 70°C, first adding dimethylol propionic acid, ethylenediamine and coupling agent KH-550 in sequence, stirring with a disperser at 800-1200 r / min for 20-30 min, then adding acetone, slowly increasing the speed of the disperser to 2000-2400 r / min, stirring for 60-90 min, and finally cooling to 60°C to obtain a hydrophilic polyurethane emulsion;
[0011] S4. Add triethylamine to the hydrophilic polyurethane emulsion, then add deionized water to dilute, stir with a disperser at 800-1200 r / min for 20-30 min, cool to room temperature, filter and package with a 200-mesh copper mesh to obtain the high-performance polyurethane coating.
[0012] Optionally, the isocyanate content of the hexamethylene diisocyanate is 23.0%, and the hydroxyl content of the polycarbonate diol is 5.0%.
[0013] Optionally, the average particle size of the hexamethylene diisocyanate is 205 nm, the viscosity of the hexamethylene diisocyanate is 600 cps, and the viscosity of the polycarbonate diol is 2500 cps.
[0014] Optionally, the ethylenediamine is replaced by hydroxyethylenediamine.
[0015] Optionally, in S2, the rotation speed of the clockwise stirring and the counterclockwise stirring is 60 r / min.
[0016] On the other hand, the present invention also provides the following technical solution: an application of a high-performance polyurethane coating, using the above-mentioned high-performance polyurethane coating, and using gas-assisted spraying to coat the high-performance polyurethane coating on the outer surface of engineering machinery.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] The invention makes it easier for the aliphatic long-chain structure of hexamethylene diisocyanate to form agglomerates by rapidly evaporating acetone at low temperature and evaporating water under reduced pressure on the prepolymer, and alternately performing clockwise stirring and counterclockwise stirring, so that the hexamethylene diisocyanate is easily wrapped by polycarbonate diol, thereby blocking the contact between the hexamethylene diisocyanate and water, effectively preventing the isocyanate and water from generating a large amount of carbon dioxide, and avoiding the formation of a large number of pinholes or bubble defects inside the high-performance polyurethane coating after film formation. The high-performance polyurethane coating has good structural strength and appearance effect after film formation. DETAILED DESCRIPTION
[0019] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] Example 1
[0021] The invention provides a high-performance polyurethane coating, which comprises the following components in parts by weight: 25 parts of hexamethylene diisocyanate, 45 parts of polycarbonate diol, 2 parts of dimethylol propionic acid, 4 parts of triethylamine, 2 parts of ethylenediamine, 0.2 parts of coupling agent KH-550, 8 parts of acetone aqueous solution, 2 parts of acetone, and 18 parts of deionized water.
[0022] The preparation method of high-performance polyurethane coating comprises the following steps:
[0023] S1. Add hexamethylene diisocyanate and polycarbonate diol into a sample preparation tank, stir at 800 r / min for 20 min at 85° C. using a disperser, and add acetone aqueous solution during stirring to obtain a prepolymer;
[0024] S2, cooling the prepolymer to room temperature and placing it in a vacuum tank, first reducing the air pressure in the vacuum tank to 37 kPa by a vacuum pump and maintaining it for 10 minutes, then reducing the air pressure in the vacuum tank to 61 kPa by a vacuum pump, and alternately stirring clockwise and counterclockwise every 1 minute for 30 minutes, finally turning off the vacuum pump and taking out the prepolymer;
[0025] S3, heating the prepolymer to 70°C, first adding dimethylolpropionic acid, ethylenediamine and coupling agent KH-550 in sequence, stirring at 800r / min for 20min with a disperser, then adding acetone, slowly increasing the speed of the disperser to 2000r / min, stirring for 60min, and finally cooling to 60°C to obtain a hydrophilic polyurethane emulsion;
[0026] S4. Add triethylamine to the hydrophilic polyurethane emulsion, then add deionized water to dilute, stir at 800 r / min for 20 min using a disperser, cool to room temperature, filter and package using a 200-mesh copper mesh to obtain a high-performance polyurethane coating.
[0027] Example 2
[0028] The present invention provides a high-performance polyurethane coating, which comprises the following components in parts by weight: 26 parts of hexamethylene diisocyanate, 50 parts of polycarbonate diol, 3 parts of dimethylol propionic acid, 5 parts of triethylamine, 3 parts of ethylenediamine, 0.3 parts of coupling agent KH-550, 10 parts of acetone aqueous solution, 3 parts of acetone, and 20 parts of deionized water;
[0029] The preparation method of high-performance polyurethane coating comprises the following steps:
[0030] S1. Add hexamethylene diisocyanate and polycarbonate diol into a sample preparation tank, stir at 85° C. with a disperser at 950 r / min for 25 min, and add acetone aqueous solution during stirring to obtain a prepolymer;
[0031] S2. Cool the prepolymer to room temperature and place it in a vacuum tank. First, reduce the air pressure in the vacuum tank to 40 kPa by a vacuum pump and maintain it for 10 minutes. Then, reduce the air pressure in the vacuum tank to 64 kPa by a vacuum pump. Stir clockwise and counterclockwise alternately every 1 minute for 30 minutes. Finally, turn off the vacuum pump and take out the prepolymer.
[0032] S3, heating the prepolymer to 70°C, first adding dimethylol propionic acid, ethylenediamine and coupling agent KH-550 in sequence, stirring at 950r / min for 25min with a disperser, then adding acetone, slowly increasing the speed of the disperser to 2100r / min, stirring for 70min, and finally cooling to 60°C to obtain a hydrophilic polyurethane emulsion;
[0033] S4. Add triethylamine to the hydrophilic polyurethane emulsion, then add deionized water to dilute, stir with a disperser at 950 r / min for 25 min, cool to room temperature, filter and package with a 200-mesh copper mesh to obtain a high-performance polyurethane coating.
[0034] Example 3
[0035] The invention provides a high-performance polyurethane coating, which comprises the following components in parts by weight: 28 parts of hexamethylene diisocyanate, 55 parts of polycarbonate diol, 3 parts of dimethylol propionic acid, 6 parts of triethylamine, 4 parts of ethylenediamine, 0.3 parts of coupling agent KH-550, 11 parts of acetone aqueous solution, 3 parts of acetone, and 22 parts of deionized water.
[0036] The preparation method of high-performance polyurethane coating comprises the following steps:
[0037] S1. Add hexamethylene diisocyanate and polycarbonate diol into a sample preparation tank, stir at 85° C. with a disperser at 1150 r / min for 25 min, and add acetone aqueous solution during stirring to obtain a prepolymer;
[0038] S2. Cool the prepolymer to room temperature and place it in a vacuum tank. First, reduce the air pressure in the vacuum tank to 45 kPa by a vacuum pump and maintain it for 10 minutes. Then, reduce the air pressure in the vacuum tank to 68 kPa by a vacuum pump. Stir clockwise and counterclockwise alternately every 1 minute for 30 minutes. Finally, turn off the vacuum pump and take out the prepolymer.
[0039] S3, heating the prepolymer to 70°C, first adding dimethylolpropionic acid, ethylenediamine and coupling agent KH-550 in sequence, stirring with a disperser at 1150r / min for 25min, then adding acetone, slowly increasing the speed of the disperser to 2300r / min, stirring for 80min, and finally cooling to 60°C to obtain a hydrophilic polyurethane emulsion;
[0040] S4. Add triethylamine to the hydrophilic polyurethane emulsion, then add deionized water to dilute, stir at 1150 r / min for 25 min using a disperser, cool to room temperature, filter and package using a 200-mesh copper mesh to obtain a high-performance polyurethane coating.
[0041] Example 4
[0042] The present invention provides a high-performance polyurethane coating, which comprises the following components in parts by weight: 30 parts of hexamethylene diisocyanate, 60 parts of polycarbonate diol, 4 parts of dimethylol propionic acid, 8 parts of triethylamine, 2-5 parts of ethylenediamine, 0.4 parts of coupling agent KH-550, 12 parts of acetone aqueous solution, 4 parts of acetone, and 24 parts of deionized water;
[0043] The preparation method of high-performance polyurethane coating comprises the following steps:
[0044] S1. Add hexamethylene diisocyanate and polycarbonate diol into a sample preparation tank, stir at 85°C with a disperser at 1200 r / min for 30 min, and add acetone aqueous solution during stirring to obtain a prepolymer.
[0045] S2. Cool the prepolymer to room temperature and place it in a vacuum tank. First, reduce the air pressure in the vacuum tank to 47 kPa by a vacuum pump and maintain it for 10 minutes. Then, reduce the air pressure in the vacuum tank to 71 kPa by a vacuum pump. Stir clockwise and counterclockwise alternately every 1 minute for 30 minutes. Finally, turn off the vacuum pump and take out the prepolymer.
[0046] S3, heating the prepolymer to 70°C, first adding dimethylol propionic acid, ethylenediamine and coupling agent KH-550 in sequence, stirring at 1200r / min for 30min with a disperser, then adding acetone, slowly increasing the speed of the disperser to 2400r / min, stirring for 90min, and finally cooling to 60°C to obtain a hydrophilic polyurethane emulsion;
[0047] S4. Add triethylamine to the hydrophilic polyurethane emulsion, then add deionized water to dilute, stir at 1200 r / min for 30 min using a disperser, cool to room temperature, filter and package using a 200-mesh copper mesh to obtain a high-performance polyurethane coating.
[0048] In Examples 1 to 4, the isocyanate content of hexamethylene diisocyanate is 23.0%, and the hydroxyl content of polycarbonate diol is 5.0%. The average particle size of hexamethylene diisocyanate is 205 nm, and the viscosity of hexamethylene diisocyanate is 600 cps, and the viscosity of polycarbonate diol is 2500 cps. In S1, when the viscosity of the prepolymer is 1900 to 2000 cps, the addition of the acetone aqueous solution is stopped. In S2, the rotation speed of the clockwise stirring and the counterclockwise stirring is 60 r / min.
[0049] In addition, in Examples 1 to 4, the volume ratios of acetone to water in the acetone aqueous solution are 2:1, 3:1, 4:1 and 4:1, respectively.
[0050] In the present invention, ethylenediamine can be replaced by hydroxyethylenediamine.
[0051] In the present invention, hexamethylene diisocyanate is an aliphatic long-chain structure. Compared with 4,4-diphenylmethane diisocyanate, isophorone diisocyanate and toluene diisocyanate, the subchain of hexamethylene diisocyanate is the most compliant, the average particle size of the prepared waterborne polyurethane is the smallest, the emulsification dispersion is easier, and the dispersion can be uniform without a large shear force. The polycarbonate diol has a linear structure, has certain elasticity and flexibility, and also has excellent heat resistance, ozone resistance and chemical corrosion resistance. The waterborne polyurethane prepared by the polycarbonate diol and hexamethylene diisocyanate has good structural strength and weather resistance.
[0052] The present invention uses acetone aqueous solution to dilute hexamethylene diisocyanate and polycarbonate diol, reduces the viscosity of the prepolymer, promotes the uniform stirring of hexamethylene diisocyanate and polycarbonate diol, and the prepolymer contains hexamethylene diisocyanate, polycarbonate diol, acetone and water to form a four-phase emulsion system. Acetone is first evaporated under reduced pressure in a vacuum tank, and while protecting the properties of hexamethylene diisocyanate and polycarbonate diol, the acetone is rapidly evaporated at low temperature, with the purpose of reducing the VOC content in the high-performance polyurethane coating. On the one hand, acetone absorbs the heat of the prepolymer during rapid low-temperature evaporation, which can reduce the sedimentation, aggregation and coagulation of water phase droplets in the prepolymer, thereby maintaining the emulsification stability of the prepolymer and facilitating the subsequent reduced-pressure evaporation of water; on the other hand, acetone causes the viscosity of the prepolymer to increase during rapid low-temperature evaporation, so that the oil phase and water phase particles are close to each other to form a compact structure, and the water-in-oil is about to be transformed into the oil-in-water. Next, water is evaporated under reduced pressure in a vacuum tank. As gaseous water leaves the prepolymer and as clockwise and counterclockwise stirring are performed alternately (slow stirring at a speed of 60 r / min), complex vortices are generated in the prepolymer, making it easier for the aliphatic long-chain structure of hexamethylene diisocyanate to wrap around hexamethylene diisocyanate to form a cluster, that is, hexamethylene diisocyanate is easily wrapped by the long-chain structure of polycarbonate diol, which can effectively block the contact between hexamethylene diisocyanate and water. A high-concentration stacked structure can be formed in the prepolymer, and unevaporated water remains in the gaps between various dispersed phases.
[0053] The invention can effectively prevent isocyanate and water from generating a large amount of carbon dioxide, and avoid forming a large number of pinholes or bubble defects inside the high-performance polyurethane coating after film formation. The high-performance polyurethane coating has good structural strength and appearance effect after film formation.
[0054] Test Example 1
[0055] Peel strength test: Take two TPU strips with a width of 1.5 cm and a length of 5 cm, polish the surface with 1500 mesh sandpaper and wipe it clean, brush one of the TPU strips with the high-performance polyurethane coating prepared in Examples 1 to 4, place it in a 50°C oven for 10 minutes, then take out the strip and stick it on the surface of another TPU strip (sticking conditions: first stick with 50kg pressure at 100°C for 2 minutes, then stick with 50kg pressure at room temperature for 6 hours) to make a sample. The sample needs to leave 3cm unsticked in order to test the clamping. On the testing machine, clamp the unsticked ends of the sample on the upper and lower clamps respectively, test the 180° peel strength with a tensile force of 500N and a peeling speed of 200mm / min, and the results are recorded in Table 1.
[0056] Table 1 Peel strength test results
[0057] 180° peel strength (N / cm) Example 1 6.02 Example 2 6.18 Example 3 6.25 Example 4 6.20
[0058] The high performance polyurethane coating prepared in Example 3 has the best 180° peel strength.
[0059] Test Example 2
[0060] Mechanical properties test: The latex film formed after drying the high-performance polyurethane coating prepared in Example 3 was taken and the mechanical properties of the latex film were measured by a universal testing machine. The results are recorded in Table 2.
[0061] Table 2 Mechanical properties test results
[0062] Universal testing machine coefficient setting 1.2 1.5 1.8 2.1 2.4 Tensile strength / MPa 11.2 16.0 18.4 22.3 22.5 Elongation at break / % 471 419 382 377 373
[0063] As shown in Table 2, as the coefficient setting of the universal testing machine increases, the tensile strength of the latex film increases, and the rate of increase slows down in the later stage; the elongation at break of the film decreases, and the rate of decrease slows down in the later stage. This is mainly due to the increase in the content of macromolecular hardness ammonia generated by the waterborne polyurethane in the polymerization reaction, while the content of the soft segment decreases, resulting in differential changes. The latex film prepared in Example 3 has a better mechanical effect overall.
[0064] The present invention provides an application of the high-performance polyurethane coating, which is coated on the outer surface of engineering machinery by gas-assisted spraying. Gas-assisted spraying can atomize the high-performance polyurethane coating into more uniform and fine droplets, which have lower surface tension than large droplets before atomization, and are conducive to the wetting, leveling and fusion of particles of the high-performance polyurethane coating, forming a defect-free high-performance coating film.
[0065] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A high performance polyurethane coating, characterized in that: The high-performance polyurethane coating comprises the following components in parts by weight: 25-30 parts of hexamethylene diisocyanate, 45-60 parts of polycarbonate diol, 2-4 parts of dimethylol propionic acid, 4-8 parts of triethylamine, 2-5 parts of ethylenediamine, 0.2-0.4 parts of coupling agent KH-550, 8-12 parts of acetone aqueous solution, 2-4 parts of acetone, and 18-24 parts of deionized water; The volume ratio of acetone to water in the acetone aqueous solution is (2-4):1; The preparation method of the high-performance polyurethane coating comprises the following steps: S1. Add hexamethylene diisocyanate and polycarbonate diol into a sample preparation tank, stir at 85° C. with a disperser at 800-1200 r / min for 20-30 min, and add acetone aqueous solution during stirring to obtain a prepolymer, the viscosity of the prepolymer is 1900-2000 cps; S2. Cool the prepolymer to room temperature and place it in a vacuum tank. First, reduce the air pressure in the vacuum tank to 37-47 kPa by a vacuum pump and maintain it for 10 minutes. Then, reduce the air pressure in the vacuum tank to 61-71 kPa by a vacuum pump. Stir clockwise and counterclockwise alternately every 1 minute for 30 minutes. Finally, turn off the vacuum pump and take out the prepolymer. S3, heating the prepolymer to 70°C, first adding dimethylol propionic acid, ethylenediamine and coupling agent KH-550 in sequence, stirring with a disperser at 800-1200 r / min for 20-30 min, then adding acetone, slowly increasing the speed of the disperser to 2000-2400 r / min, stirring for 60-90 min, and finally cooling to 60°C to obtain a hydrophilic polyurethane emulsion; S4. Add triethylamine to the hydrophilic polyurethane emulsion, then add deionized water to dilute, stir with a disperser at 800-1200 r / min for 20-30 min, cool to room temperature, filter and package with a 200-mesh copper mesh to obtain the high-performance polyurethane coating.
2. A high performance polyurethane coating according to claim 1, characterized in that: The isocyanate content of the hexamethylene diisocyanate is 23.0%, and the hydroxyl content of the polycarbonate diol is 5.0%.
3. A high performance polyurethane coating according to claim 2, characterized in that: The average particle size of the hexamethylene diisocyanate is 205 nm, the viscosity of the hexamethylene diisocyanate is 600 cps, and the viscosity of the polycarbonate diol is 2500 cps.
4. A high performance polyurethane coating according to claim 1, characterized in that: The ethylenediamine is replaced by hydroxyethylenediamine.
5. A high performance polyurethane coating according to claim 1, characterized in that: In S2, the rotation speed of the clockwise stirring and the counterclockwise stirring is 60 r / min.
6. An application of a high-performance polyurethane coating, using the high-performance polyurethane coating as claimed in any one of claims 1 to 5, characterized in that: The high-performance polyurethane coating is coated on the outer surface of the engineering machinery by gas-assisted spraying.
Citation Information
Patent Citations
Double cross-linking waterborne polyurethane self-extinction resin and preparation method thereof
CN107200823A
Super-thick composite-free polyurethane synthetic leather and preparation method thereof
CN112593418A
High-solid-content low-temperature anti-cracking single-component waterborne polyurethane waterproof coating and preparation method thereof
CN115286992A
Waterborne polyurethane coating and preparation method thereof
CN115449281A
Preparation method of waterborne polyurethane with solid content of 60%
CN116970138A
Cited By
Silicon dioxide enhanced high-corrosion-resistance waterborne polyurethane coating and preparation method thereof
CN120173503A