Natural raw lacquer coating suitable for ancient building construction and preparation method and construction method thereof

By mixing natural raw paint with anhydrous micro-nano aluminosilicate and ammonium salts and combining natural raw paint coatings prepared by special processes, the existing antique architectural raw paint coatings have solved the problems of poor UV resistance and insufficient substrate adaptability, and achieved the Better weather resistance, alkali resistance and wear resistance improve the decoration and protection effect of ancient building construction.

CN118931391AInactive Publication Date: 2024-11-12LICHUAN DELONG LACQUER TECH CO LTD +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411241946.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2020-07-17
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing antique architectural raw paint coatings have shortcomings in terms of poor UV resistance, large substrate selectivity, high requirements for coating film formation, adhesion, weather resistance, alkali resistance, wear resistance, flame retardancy, etc., which are difficult to meet the ancient times. Building construction needs.

Method used

By mixing natural raw paint with mixed blank oil, anhydrous micro-nano aluminosilicate and ammonium salt in a specific proportion and mixing with special processes, natural raw paint coatings with improved viscosity and performance are prepared. They are suitable for the construction of ancient buildings and are adopted Construction methods for spraying, rolling, brushing or scraping.

Benefits of technology

Improve the weather resistance, alkali resistance, wear resistance and flame retardancy of the paint, enhance the adaptability of the substrate, significantly improve the performance and protection effect of paint decoration in ancient buildings, and maintain the original style and environmental protection of raw paint. characteristic.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005029549490000041
    Figure BDA0005029549490000041
  • Figure BDA0005029549490000061
    Figure BDA0005029549490000061
  • Figure BDA0005029549490000071
    Figure BDA0005029549490000071
Patent Text Reader

Abstract

The invention relates to a natural raw lacquer coating suitable for ancient building construction and a preparation method and a construction method thereof, and the preparation method comprises the following steps: mixing tung oil and stillingia oil, and boiling to required viscosity to form mixed blank oil; the mixed blank oil, pure natural raw lacquer, anhydrous micro-nano aluminosilicate and ammonium salt are put into a container according to the proportion to be kneaded, and paint is formed; the preparation method comprises the following steps: mixing furfuryl alcohol, ethyl lactate and turpentine in proportion to form a mixed solvent, adding a proper amount of the mixed solvent into paint to adjust the viscosity to specified requirements, and then filtering to obtain the natural raw lacquer coating suitable for ancient building repair.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the invention patent with application date of July 17, 2020, application number 202010688260.8, and invention name "A natural raw lacquer coating specially used for the construction of ancient buildings and its preparation method". Technical Field

[0002] The invention relates to a natural raw lacquer coating suitable for the repair of ancient buildings and a preparation method and a construction method thereof. Background Art

[0003] The decorative effect of paint on the surface of objects is well known. It can increase the color and gloss of the surface of objects, and can also modify and smooth the roughness and defects of the surface of objects, improve the appearance quality, increase the product value, and extend the service life of objects.

[0004] Natural lacquer is one of the native products of my country. It comes from the original forest and the natural lacquer tree family. Natural lacquer is the natural lacquer tree liquid cut from the lacquer tree. The natural lacquer liquid mainly contains high molecular lacquer phenol, laccase, gum and water. Natural lacquer is known as the "three treasures" of my country (tree cutting lacquer, silkworm spinning silk, bee making honey), and is also recognized as the "king of paint" in the world. Because natural lacquer has the properties of corrosion resistance, penetration resistance, moisture resistance, mildew resistance, acid resistance, etc., the paint film has the characteristics of strong hardness and wear resistance, and has a beautiful and durable luster, so raw lacquer is widely used in defense and military industry, chemical industry, petroleum industry, metallurgical mining industry, textile printing and dyeing industry, pharmaceutical industry, and the protection of ancient buildings and cultural relics. With the changes in the needs of modern industry and life, problems have arisen in the application of raw lacquer: raw lacquer has poor UV resistance (i.e., poor UV resistance), and the materials decorated with raw lacquer are not suitable for outdoor use. Therefore, at present, there is an urgent need for a raw lacquer with strong anti-aging performance, good mechanical properties and a wide range of applications.

[0005] Raw lacquer, also known as national lacquer, lacquer, earth lacquer, and old lacquer, is widely used in antique architectural paint projects for its simple and dignified, warm and elegant, strong and corrosion-resistant, and ecological and energy-saving decorative style. It has a history of more than 2,500 years and has left many famous buildings from ancient times to the present. However, natural raw lacquer is harvested from lacquer trees. Due to the influence of factors such as variety, soil, and climate, the quality and performance vary greatly and are uneven. Certain technical means must be adopted for processing to meet the construction and decoration requirements. Existing antique architectural raw lacquer coatings have many shortcomings, such as large selectivity for substrates, high requirements for coating film-forming conditions, poor adhesion, weather resistance, alkali resistance, wear resistance, and flame retardancy. Summary of the invention

[0006] The purpose of the present invention is to provide a natural raw lacquer coating suitable for the construction of ancient buildings and a preparation method and a construction method thereof.

[0007] The present invention provides a method for preparing a natural lacquer coating suitable for the construction of ancient buildings, which comprises the following steps:

[0008] a) Mixed stock oil preparation: 4 parts by mass of catalpa oil and 6 parts by mass of tung oil are put into a reaction pot and mixed evenly, heated to 180°C, kept warm for 40 minutes, stirred with a long-handled spoon to exhaust smoke, and then continued to heat to 200°C-220°C, sampled and tested the viscosity every 10 minutes, when the temperature reached 230°C-240°C and the viscosity reached 45000000mpa·s, stopped heating, transferred to another container, stirred and cooled to obtain mixed stock oil;

[0009] b) Preparation of mixed solvent: 5 parts by mass of turpentine, 2 parts by mass of ethyl lactate and 3 parts by mass of furfuryl alcohol were stirred in a container for 5 minutes to obtain a mixed solvent;

[0010] c) paint preparation: 56 parts by weight of natural raw lacquer with a content of 70% and 44 parts by weight of the mixed base oil are put into a kneader, and 15%-20% of anhydrous micro-nano aluminosilicate and 2‰-5‰ of ammonium salt by weight of the paint are added and kneaded for 2 hours;

[0011] d) Viscosity adjustment: add 15%-20% of the mixed solvent by weight of the paint and stir evenly, adjust the viscosity of the T4 cup to 180-200 seconds and filter to obtain the natural raw lacquer coating.

[0012] In the present invention, the weight of the lacquer in step c) is the total weight of natural raw lacquer and mixed base oil.

[0013] In the present invention, the weight of the paint in step d) is the total weight of natural raw lacquer, mixed base oil, anhydrous micro-nano aluminosilicate and ammonium salt.

[0014] In the present invention, the catalpa oil is the catalpa oil extracted from the seed kernels of the Chinese tallow tree; and the tung oil is the tung nut oil extracted from the seeds of the tung nut tree.

[0015] In the present invention, the natural raw lacquer is the raw lacquer obtained by scratching the bast of Rhus verniciflua;

[0016] The natural raw lacquer includes one or a mixture of raw lacquer from various raw lacquer producing areas in China.

[0017] Preferably, the anhydrous micro-nano aluminosilicate is ultrapure anhydrous micro-nano aluminosilicate, spherical in shape, and 20 μm in particle size. Anhydrous micro-nano aluminosilicate is an ultrafine and ultrapure material with good insulation, flame retardancy, thermal stability, acid and alkali resistance, weather resistance and wear resistance.

[0018] The present invention also provides a natural raw lacquer coating obtained by the modulation method described in the above technical solution, wherein the natural raw lacquer coating has a viscosity of 180S, a solid content of 62%, and a fineness of 5 microns.

[0019] The present invention also provides a construction method for the natural raw lacquer coating described in the above technical solution, including spraying, rolling, brushing or scraping.

[0020] Preferably, the wet paint film thickness obtained after the construction of the natural raw lacquer paint is 25 to 35 microns.

[0021] Preferably, the construction interface of the natural raw lacquer coating includes concrete, wood or steel.

[0022] In the present invention, the kneading machine is a special machine for solving the problem of mixing high-viscosity materials.

[0023] In the present invention, the Chinese tallow tree used is:

[0024] Sapium sebiferum (L.) Roxb. is a deciduous tree of the Euphorbiaceae family and the genus Sapium. Sapium sebiferum is a colorful tree with bright red leaves in spring and autumn, which are as bright as red maple. It is an economic tree species unique to China and has a cultivation history of more than 1,400 years. Sapium sebiferum has a strong adaptability to soil and can grow in red soil, yellow soil, yellow-brown soil, purple soil, brown soil and other soil types, from sand to clay, and in acidic, neutral or slightly alkaline soils. It is one of the tree species with strong salt resistance.

[0025] Tung oil requires high soil moisture and can tolerate short-term waterlogging. It also has a certain degree of wind resistance and is more resistant to drought and early barrenness. In addition, Tung oil has a strong resistance to toxic hydrogen fluoride gas. Tung oil has economic and horticultural value. The wax on the outer coat of the seeds is called "tung wax", which can be extracted into "skin oil" for making high-grade soaps, wax paper, candles, etc. The oil extracted from the kernel is called "tung oil" or "green oil", which is used for paints, inks, etc. The aril is the raw material for making candles and soaps, and has extremely high economic value. Its wood is also a good quality wood.

[0026] The Chinese tallow tree has extremely high ornamental value.

[0027] The invention provides a method for preparing a natural raw lacquer coating suitable for the construction of ancient buildings, comprising the following materials and steps: firstly, tung oil and catalpa oil are mixed, and the mixture is boiled to a required viscosity to form a mixed germ oil; the mixed germ oil, pure natural raw lacquer, anhydrous micro-nano aluminosilicate, and ammonium salt are put into a container in proportion and kneaded to form a lacquer; furfuryl alcohol, ethyl lactate, and turpentine are mixed in proportion to form a mixed solvent, an appropriate amount of the mixed solvent is added to the lacquer to adjust the viscosity to a specified requirement, and then filtered to obtain the natural raw lacquer coating.

[0028] The quality indicators of the natural lacquer coating provided by the present invention are shown in Table 1 below:

[0029] Table 1 Quality indexes of natural lacquer coatings

[0030] Serial number project Standard indicators Sample indicators Detection Methods 1 State of paint in container Uniform, no lumps or foreign matter Uniform, no lumps or foreign matter Visual inspection 2 Viscosity 180S 180S GB / T1723-1993 3 Solid content% 48 62 GB / T1725-2007 4 Fineness (micrometer) ≤5 5 GB / T1724-1993 5 Storage stabilizer (℃) month 6 6 GB6753.3

[0031] The product of the present invention is suitable for various ancient building components, such as concrete, wood, steel, etc. The construction method is to adopt one of spraying, rolling, brushing, and scraping. The product of the present invention is evenly coated on a flat and clean surface, and the wet paint film thickness is 25-35 microns. After 7 days, the test is performed. The paint film performance effect is shown in Table 2:

[0032] Table 2 Paint film performance effect

[0033]

[0034] The beneficial effects of the natural lacquer coating provided by the present invention are:

[0035] The invention adds mixed base oil and micro-nano aluminum silicate and ammonium salt to pure natural raw lacquer (Rawlaequer), and adopts a special process to prepare a raw lacquer coating suitable for the repair of ancient buildings. The coating maintains the original style of raw lacquer decoration, and adds the functions of weather resistance, alkali resistance, wear resistance, flame retardancy, etc. required for the repair of ancient buildings and the paint decoration of antique buildings. The coating provided by the invention has strong adaptability to the substrate, low requirements for film forming conditions, and well solves various problems in the paint decoration process of the repair of ancient buildings.

[0036] The paint film performance of the paint used for the construction of ancient buildings prepared by using natural raw lacquer is obviously better than that of the existing similar paints, and has excellent protective and decorative performance for ancient buildings and newly built antique buildings. Natural raw lacquer, catalpa oil and tung oil are used as raw materials. These raw materials come from plants, are green and environmentally friendly, ecological and energy-saving, and recyclable. DETAILED DESCRIPTION

[0037] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0038] Example 1

[0039] (I) Preparation of mixed stock oil: Take 4 parts of catalpa oil and 6 parts of tung oil, put them into a reaction pot and mix them evenly, heat to 180℃, keep warm for 40 minutes, stir with a long-handled spoon to exhaust smoke, then continue to heat to 200℃-220℃, take samples every 10 minutes to test the viscosity, when the temperature reaches 230℃-240℃ and the viscosity reaches 45000000mPa·s, stop heating, transfer to another container, stir and cool to make mixed stock oil.

[0040] (ii) Preparation of mixed solvent: Take 5 parts of turpentine oil, 2 parts of ethyl lactate and 3 parts of furfuryl alcohol and stir them in a container for 5 minutes to obtain a mixed solvent.

[0041] (III) Paint preparation: 56 parts of Hubei Maoba raw paint with a content of 70% and 44 parts of mixed base oil are put into a kneading machine, and 15%-20% of anhydrous micro-nano aluminosilicate and 2‰-5‰ ammonium salt by weight of the paint are added and kneaded for 2 hours;

[0042] (IV) Viscosity adjustment: Add 15%-20% of the paint weight of the mixed solvent and stir evenly, adjust the viscosity to 180-200 seconds (T4 cup) and filter. The quality indicators of natural raw lacquer coatings are as follows Table 3:

[0043] Table 3 Quality indexes of natural lacquer coatings

[0044] Serial number project Standard indicators Sample indicators Detection Methods 1 State of paint in container Uniform, no lumps or foreign matter Uniform, no lumps or foreign matter Visual inspection 2 Viscosity 180S 180S GB / T1723-1993 3 Solid content% 48 62 GB / T1725-2007 4 Fineness (micrometer) ≤5 5 GB / T1724-1993 5 Storage stabilizer (℃) month 6 6 GB6753.3

[0045] (V) The product of the present invention is suitable for various ancient building components, such as concrete, wood, steel, etc. The construction method is to adopt one of spraying, rolling, brushing, and scraping. The product of the present invention is evenly coated on a flat and clean surface, and the wet paint film thickness is 25-35 microns. After 7 days, the test is performed. The paint film performance effect is shown in Table 4:

[0046] Table 4 Paint film performance effect

[0047]

[0048] Example 2

[0049] (I) Preparation of mixed stock oil: Take 4 parts of catalpa oil and 6 parts of tung oil, put them into a reaction pot and mix them evenly, heat to 180℃, keep warm for 40 minutes, stir with a long-handled spoon to exhaust smoke, then continue to heat to 200℃-220℃, take samples every 10 minutes to test the viscosity, when the temperature reaches 230℃-240℃ and the viscosity reaches 45000000mPa·s, stop heating, transfer to another container, stir and cool to make mixed stock oil.

[0050] (ii) Preparation of mixed solvent: Take 5 parts of turpentine oil, 2 parts of ethyl lactate and 3 parts of furfuryl alcohol and stir them in a container for 5 minutes to obtain a mixed solvent.

[0051] (III) Paint preparation: 56 parts of Shaanxi Pingli raw paint with a content of 70% and 44 parts of mixed base oil are put into a kneading machine, and 15%-20% of anhydrous micro-nano aluminosilicate and 2‰-5‰ ammonium salt by weight of the paint are added and kneaded for 2 hours;

[0052] (IV) Viscosity adjustment: Add 15%-20% of the paint weight of the mixed solvent and stir evenly, adjust the viscosity to 180-200 seconds (T4 cup) and filter. The quality indicators of natural raw lacquer coatings are as follows Table 5:

[0053] Table 5 Quality indexes of natural lacquer coatings

[0054] Serial number project Standard indicators Sample indicators Detection Methods 1 State of paint in container Uniform, no lumps or foreign matter Uniform, no lumps or foreign matter Visual inspection 2 Viscosity 180S 180S GB / T1723-1993 3 Solid content% 48 62 GB / T1725-2007 4 Fineness (micrometer) ≤5 5 GB / T1724-1993 5 Storage stabilizer (℃) month 6 6 GB6753.3

[0055] (V) The product of the present invention is suitable for various ancient building components, such as concrete, wood, steel, etc. The construction method is to adopt one of spraying, rolling, brushing, and scraping. The product of the present invention is evenly coated on a flat and clean surface, with a wet paint film thickness of 25-35 microns, and tested after 7 days. The paint film performance effect is shown in Table 6:

[0056] Table 6 Paint film performance effect

[0057]

[0058]

[0059] Example 3

[0060] (I) Preparation of mixed stock oil: Take 4 parts of catalpa oil and 6 parts of tung oil, put them into a reaction pot and mix them evenly, heat to 180℃, keep warm for 30 minutes, stir with a long-handled spoon to exhaust smoke, then continue to heat to 200℃-220℃, take samples every 10 minutes to test the viscosity, when the temperature reaches 230℃-240℃ and the viscosity reaches 45000000mPa·s, stop heating, transfer to another container, stir and cool to make mixed stock oil.

[0061] (ii) Preparation of mixed solvent: Take 5 parts of turpentine oil, 2 parts of ethyl lactate and 3 parts of furfuryl alcohol and stir them in a container for 5 minutes to obtain a mixed solvent.

[0062] (III) Paint preparation: 56 parts of Guizhou Bijie raw lacquer with a content of 70% and 44 parts of mixed base oil are put into a kneading machine, and 15%-20% of anhydrous micro-nano silicate and 2‰-5‰ ammonium salt by weight of the paint are added and kneaded for 2 hours;

[0063] (IV) Viscosity adjustment: Add 15%-20% of the paint weight of the mixed solvent and stir evenly, adjust the viscosity to 180-200 seconds (T4 cup) and filter. The quality indicators of natural lacquer coatings are as follows Table 7:

[0064] Table 7 Quality indexes of natural lacquer coatings

[0065] Serial number project Standard indicators Sample indicators Detection Methods 1 State of paint in container Uniform, no lumps or foreign matter Uniform, no lumps or foreign matter Visual inspection 2 Viscosity 180S 180S GB / T1723-1993 3 Solid content% 48 62 GB / T1725-2007 4 Fineness (micrometer) ≤5 5 GB / T1724-1993 5 Storage stabilizer (℃) month 6 6 GB6753.3

[0066] (V) The product of the present invention is suitable for various ancient building components, such as concrete, wood, steel, etc. The construction method is to adopt one of spraying, rolling, brushing, and scraping. The product of the present invention is evenly coated on a flat and clean surface, with a wet paint film thickness of 25-35 microns, and tested after 7 days. The paint film performance effect is shown in Table 8:

[0067] Table 8 Paint film performance effect

[0068]

[0069] Example 4

[0070] (I) Preparation of mixed stock oil: Take 4 parts of catalpa oil and 6 parts of tung oil, put them into a reaction pot and mix them evenly, heat to 180℃, keep warm for 30 minutes, stir with a long-handled spoon to exhaust smoke, then continue to heat to 200℃-220℃, take samples every 10 minutes to test the viscosity, when the temperature reaches 230℃-240℃ and the viscosity reaches 45000000mPa·s, stop heating, transfer to another container, stir and cool to make mixed stock oil.

[0071] (ii) Preparation of mixed solvent: Take 5 parts of turpentine oil, 2 parts of ethyl lactate and 3 parts of furfuryl alcohol and stir them in a container for 5 minutes to obtain a mixed solvent.

[0072] (III) lacquer preparation: 25 parts of each of 70% Hubei Maoba lacquer, Shaanxi Pingli lacquer, Guizhou Bijie lacquer and Chongqing Chengkou lacquer are mixed evenly, then 56 parts of the mixed lacquer and 44 parts of mixed base oil are put into a kneader, 15%-20% of the lacquer weight of anhydrous micro-nano silicate and 2‰-5‰ of ammonium salt are added and kneaded for 2 hours;

[0073] (IV) Viscosity adjustment: Add 15%-20% of the paint weight of the mixed solvent and stir evenly, adjust the viscosity to 180-200 seconds (T4 cup) and filter. The quality indicators of natural lacquer coatings are as follows Table 9:

[0074] Table 9 Quality indexes of natural lacquer coatings

[0075] Serial number project Standard indicators Sample indicators Detection Methods 1 State of paint in container Uniform, no lumps or foreign matter Uniform, no lumps or foreign matter Visual inspection 2 Viscosity 180S 180S GB / T1723-1993 3 Solid content% 48 62 GB / T1725-2007 4 Fineness (micrometer) ≤5 5 GB / T1724-1993 5 Storage stabilizer (℃) month 6 6 GB6753.3

[0076] (V) The product of the present invention is suitable for various ancient building components, such as concrete, wood, steel, etc. The construction method is to adopt one of spraying, rolling, brushing, and scraping. The product of the present invention is evenly coated on a flat and clean surface, and the wet paint film thickness is 25-35 microns. After 7 days, the test is performed. The paint film performance effect is shown in Table 10:

[0077] Table 10 Paint film performance effect

[0078]

[0079]

[0080] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a natural lacquer coating suitable for the construction of ancient buildings. It is characterized in that It consists of the following steps: a) Mixed stock oil preparation: 4 parts by mass of catalpa oil and 6 parts by mass of tung oil are put into a reaction pot and mixed evenly, heated to 180°C, kept warm for 40 minutes, stirred with a long-handled spoon to exhaust smoke, and then continued to heat to 200°C-220°C, sampled and tested the viscosity every 10 minutes, when the temperature reached 230°C-240°C and the viscosity reached 45000000mpa·s, stopped heating, transferred to another container, stirred and cooled to obtain mixed stock oil; b) Preparation of mixed solvent: 5 parts by mass of turpentine, 2 parts by mass of ethyl lactate and 3 parts by mass of furfuryl alcohol were stirred in a container for 5 minutes to obtain a mixed solvent; c) paint preparation: 56 parts by weight of natural raw lacquer with a content of 70% and 44 parts by weight of the mixed base oil are put into a kneader, and 15%-20% of anhydrous micro-nano aluminosilicate and 2‰-5‰ of ammonium salt by weight of the paint are added and kneaded for 2 hours; d) Viscosity adjustment: add 15%-20% of the mixed solvent by weight of the paint and stir evenly, adjust the viscosity of the T4 cup to 180-200 seconds and filter to obtain the natural raw lacquer coating.

2. The modulation method according to claim 1, It is characterized in that The anhydrous micro-nano aluminosilicate is ultrapure anhydrous micro-nano aluminosilicate, has a spherical shape, and a particle size of 20 μm.

3. The natural lacquer coating obtained by the preparation method according to claim 1 or 2, It is characterized in that The natural lacquer coating has a viscosity of 180S, a solid content of 62%, and a fineness of 5 microns.

4. The construction method of the natural lacquer coating according to claim 3, It is characterized in that Application may include spraying, rolling, brushing or scraping.

5. The construction method according to claim 4, It is characterized in that The wet paint film thickness obtained after the natural raw lacquer coating is applied is 25 to 35 microns.

6. The construction method according to claim 4, It is characterized in that The construction interface of the natural raw lacquer coating includes concrete, wood or steel.

Citation Information

Patent Citations

  • Wear resistant raw lacquer coating for mineral dressing equipment concentrating table and preparation thereof

    CN101302398A

  • Preparation of natural anti-rust lacquer

    CN101348691A

  • Preparation method of furniture paint

    CN110862768A

  • Japanese lacquer-based coating, method for producing the same, and japanese lacquer-coated material

    JP2008001785A