Wear-resistant self-lubricating diamond-like carbon-based composite coating as well as preparation method and application thereof

By depositing the gradient multi-layer coating of the Cr layer, CrN layer and alternately arranged DLC-B4C-WC/DLC-MoS2 composite layer on the aerospace equipment components, the wear resistance and self-responsiveness of aerospace equipment components is solved in harsh environments. The problem of insufficient lubricity has achieved high hardness, low friction coefficient and long service life.

CN118932287AActive Publication Date: 2024-11-12SOUTH CHINA UNIV OF TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410992037.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

The driving mechanism of aerospace equipment is prone to problems such as bite, surface scratches, and sticking wear in harsh environments such as high vacuum and strong radiation, resulting in a shortening of the service life of parts. The existing diamond-like films are graphitized at high temperatures, and their hardness is and wear resistance decreases and short service life.

Method used

A wear-resistant self-lubricating diamond-like composite coating consisting of a Cr layer, a CrN layer and a functional layer is adopted. The functional layer includes an alternately arranged DLC-B4C-WC composite layer and a DLC-MoS2 composite layer, and is subject to magnetron sputtering technology. Deposition on the surface of the metal matrix, a gradient multilayer coating is formed to improve hardness and self-lubricating properties.

Benefits of technology

It realizes a coating with high hardness, low friction coefficient, self-lubricating and long service life under high vacuum environments, overcomes the problem of mismatch between the coating and the substrate performance, and significantly improves the operating reliability and stability of aerospace equipment components. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932287A_ABST
    Figure CN118932287A_ABST
Patent Text Reader

Abstract

The invention discloses a wear-resistant self-lubricating diamond-like carbon-based composite coating as well as a preparation method and application thereof. The wear-resistant self-lubricating diamond-like carbon-based composite coating comprises a Cr layer, a CrN layer and a functional layer which are sequentially arranged in a stacked mode, the functional layer comprises a plurality of DLC-B4C-WC composite layers and a plurality of DLC-MoS2 composite layers, the DLC-B4C-WC composite layers and the DLC-MoS2 composite layers are alternately arranged, the layer, closest to the CrN layer, of the functional layer is the DLC-B4C-WC composite layer, and the layer, closest to the CrN layer, of the functional layer is the DLC-MoS2 composite layer. And the layer farthest from the CrN layer is a DLC-MoS2 composite layer. The wear-resistant self-lubricating diamond-like carbon-based composite coating has the advantages of high hardness, low friction coefficient, self-lubrication, long service life and the like, can be used as a surface protective coating of key parts of a driving mechanism to improve the operation reliability and stability of aerospace equipment, and is suitable for large-scale industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of surface treatment, and in particular to a wear-resistant self-lubricating diamond-like carbon-based composite coating and a preparation method and application thereof. Background Art

[0002] The driving mechanism of aerospace equipment needs to be exposed to harsh environments such as high vacuum, strong radiation, atomic oxygen erosion, high and low temperature alternation, etc. for a long time, which is prone to problems such as seizure, surface scratches, and adhesive wear, which will seriously affect the service life of the transmission parts of the driving mechanism. Therefore, it is urgent to perform surface treatment on the parts of aerospace equipment to improve their wear resistance and self-lubrication, thereby extending the service life of the parts.

[0003] Research has found that by using physical vapor deposition technology (e.g. magnetron sputtering) to deposit wear-resistant / self-lubricating coatings on the surface of drive mechanism components, the performance and service life of the components can be improved without affecting the size and shape of the components. Diamond-like carbon (DLC) films have the advantages of high hardness, excellent wear resistance, and good chemical stability. They have good application prospects in improving the service life of components of drive mechanisms of aerospace equipment. However, DLC films have disadvantages such as poor thermal stability and poor environmental adaptability. They will gradually undergo graphitization at higher temperatures, resulting in a significant decrease in their hardness and wear resistance. In addition, DLC films will also suffer from severe adhesive wear in a high vacuum environment, resulting in a short service life.

[0004] Therefore, it is of great significance to develop a diamond-like carbon-based coating with high hardness, low friction coefficient, self-lubrication and long service life. Summary of the invention

[0005] The purpose of the present invention is to provide a wear-resistant self-lubricating diamond-like carbon-based composite coating and a preparation method and application thereof.

[0006] The technical solution adopted by the present invention is:

[0007] A wear-resistant and self-lubricating diamond-like carbon-based composite coating, comprising a Cr layer, a CrN layer and a functional layer stacked in sequence; the functional layer comprises a plurality of DLC-B4C-WC composite layers and a plurality of DLC-MoS2 composite layers, and the DLC-B4C-WC composite layers and the DLC-MoS2 composite layers are alternately arranged; the layer closest to the CrN layer in the functional layer is the DLC-B4C-WC composite layer, and the layer farthest from the CrN layer is the DLC-MoS2 composite layer.

[0008] Preferably, the thickness of the Cr layer is 0.1 μm to 0.2 μm.

[0009] Preferably, the thickness of the CrN layer is 0.1 μm to 0.2 μm.

[0010] Preferably, the thickness of the functional layer is 1.5 μm to 5 μm.

[0011] Preferably, the thickness of the DLC-B4C-WC composite layer is 0.01 μm to 0.3 μm.

[0012] Preferably, the thickness of the DLC-MoS2 composite layer is 0.01 μm to 0.3 μm.

[0013] A method for preparing the wear-resistant self-lubricating diamond-like carbon-based composite coating as described above comprises the following steps:

[0014] 1) In a protective atmosphere, Cr is deposited on the surface of a metal substrate by DC magnetron sputtering a Cr target to form a Cr layer;

[0015] 2) In a protective atmosphere containing nitrogen, CrN is deposited on the surface of the Cr layer by DC magnetron sputtering of a Cr target to form a CrN layer;

[0016] 3) In a protective atmosphere, DLC, B4C and WC are deposited on the surface of the CrN layer by high-power pulsed magnetron sputtering of graphite target, B4C target and WC target to form a DLC-B4C-WC composite layer;

[0017] 4) In a protective atmosphere, DLC and MoS2 are deposited on the surface of the DLC-B4C-WC composite layer by medium frequency magnetron sputtering of a graphite target and a MoS2 target to form a DLC-MoS2 composite layer;

[0018] 5) Repeat the operations of step 3) and step 4) to alternately deposit DLC-B4C-WC composite layers and DLC-MoS2 composite layers to form a functional layer, thereby obtaining a wear-resistant and self-lubricating diamond-like carbon-based composite coating.

[0019] Preferably, the protective atmosphere in step 1) is an argon atmosphere.

[0020] Preferably, the metal matrix in step 1) is one of a 2Cr13 martensitic stainless steel matrix, a 05Cr17Ni4Cu4Nb martensitic stainless steel matrix, and a YG6 cemented carbide matrix.

[0021] Preferably, the purity of the Cr target in step 1) is higher than 99.95%.

[0022] Preferably, the DC magnetron sputtering in step 1) is carried out under the conditions of a working gas pressure of 0.4Pa to 1.0Pa and a Cr target current of 1.0A to 3.0A.

[0023] Preferably, the metal substrate in step 1) is pretreated before use, and the pretreatment comprises the following steps:

[0024] a) grinding and polishing the surface of the metal substrate (removing the oxide film on the surface);

[0025] b) The metal substrate is ultrasonically cleaned with acetone and anhydrous ethanol for 10 to 20 minutes each (to remove grease and pollutants on the surface and make the surface of the metal substrate smooth), blown dry, and then placed in a protective atmosphere and Ar-ionized on the surface of the substrate using an anode layer ion source. + Etching (removing pollutants and oxide layers on the surface of the metal substrate, thereby improving the bonding strength between the metal substrate and the coating).

[0026] Preferably, in step b) Ar + The etching is performed under the condition of a bias voltage of -1000V to -800V.

[0027] Preferably, the nitrogen-containing protective atmosphere in step 2) is a nitrogen-argon mixed atmosphere.

[0028] Preferably, the purity of the Cr target in step 2) is higher than 99.95%.

[0029] Preferably, the DC magnetron sputtering in step 2) is carried out under the conditions of a working gas pressure of 0.8Pa to 1.0Pa and a Cr target current of 1.0A to 3.0A.

[0030] Preferably, the protective atmosphere in step 3) is an argon atmosphere.

[0031] Preferably, the purity of the B4C target material in step 3) is higher than 99.5%, and the B content is 85% to 90%.

[0032] Preferably, in step 3), the purity of the WC target is higher than 99.5%, and the W content is 90% to 95%.

[0033] Preferably, the high-power pulsed magnetron sputtering in step 3) is carried out under the conditions of a working gas pressure of 0.5Pa to 1.0Pa, an average sputtering power of 2.0kW to 6.0kW, and a bias voltage of -350V to 0V.

[0034] Preferably, the protective atmosphere in step 4) is an argon atmosphere.

[0035] Preferably, the medium frequency magnetron sputtering in step 4) is carried out under the conditions of a working gas pressure of 0.5Pa to 1.0Pa, an average sputtering power of 0.5kW to 3.0kW, and a bias voltage of -350V to 0V.

[0036] A space equipment comprises the above-mentioned wear-resistant self-lubricating diamond-like carbon-based composite coating.

[0037] The beneficial effects of the present invention are as follows: the wear-resistant and self-lubricating diamond-like carbon-based composite coating of the present invention has the advantages of high hardness, low friction coefficient, self-lubrication, long service life, etc. It can be used as a surface protective coating for key components of a drive mechanism to improve the operational reliability and stability of aerospace equipment, and is suitable for large-scale industrial applications.

[0038] Specifically:

[0039] 1) The wear-resistant and self-lubricating diamond-like carbon-based composite coating of the present invention comprises a Cr layer, a CrN layer and a functional layer which are stacked in sequence, wherein the Cr layer is used to regulate the compatibility of the metal substrate surface, the CrN layer focuses on connecting the upper and lower parts, enhancing the film-substrate bonding force, and buffering and eliminating the residual internal stress between the metal substrate and the coating, thereby improving the impact resistance of the composite coating, so that the functional layer can be effectively combined with the metal substrate surface, and the functional layer is not easy to break and fall off during friction, the DLC-B4C-WC composite layer in the functional layer is used to give the composite coating high hardness and wear resistance, and the DLC-MoS2 composite layer in the functional layer is used to give the composite coating self-lubricating and low friction characteristics, so that the composite coating finally has the advantages of high hardness, low friction coefficient, self-lubricating, long service life, etc., which can well meet the practical application requirements in the aerospace field;

[0040] 2) The present invention adopts a gradient multi-layer coating design, which overcomes the problem of performance mismatch between the coating and the substrate, alleviates the stress of the coating itself and between the coatings to the greatest extent, reduces the generation of cracks, and improves the bonding strength between the coating and the substrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 It is a schematic structural diagram of the wear-resistant self-lubricating diamond-like carbon-based composite coating of the present invention.

[0042] Description of the accompanying drawings: 10, metal substrate; 20, Cr layer; 30, CrN layer; 40, functional layer; 401, DLC-B4C-WC composite layer; 402, DLC-MoS2 composite layer.

[0043] Figure 2 This is a relationship curve between the friction coefficient and the number of friction cycles of the wear-resistant self-lubricating diamond-like carbon-based composite coating of Example 1. DETAILED DESCRIPTION

[0044] The present invention will be further explained and illustrated below in conjunction with specific embodiments.

[0045] Embodiment 1:

[0046] A wear-resistant self-lubricating diamond-like carbon-based composite coating (schematic diagram of the structure as shown in Figure 1 The preparation method thereof is as follows:

[0047] 1) The surface of the 2Cr13 martensitic stainless steel substrate was ground and polished, and then ultrasonically cleaned with acetone and anhydrous ethanol for 15 min each, dried, and then placed on the workpiece rotating rack of the magnetron sputtering coating chamber. The magnetron sputtering coating chamber was evacuated to a pressure below 3×10 -3 Pa, and then argon gas was introduced, and the negative bias voltage of the workpiece support was adjusted to -800 V. The 2Cr13 martensitic stainless steel substrate was cleaned and etched by the anode layer ion source, and the magnetron sputtering coating chamber was evacuated to a pressure below 3×10 -3 Pa, then introduce argon gas to a pressure of 0.42Pa, and then magnetron sputter Cr target (purity higher than 99.95%) to deposit Cr on the surface of 2Cr13 martensitic stainless steel substrate, the distance between 2Cr13 martensitic stainless steel substrate and Cr target is 60cm, the current of Cr target is 3.0A, and a Cr layer (thickness is 0.2μm) is formed;

[0048] 2) maintaining the argon flow rate and introducing 50 sccm of nitrogen, adjusting the flow rates of argon and nitrogen to maintain the working pressure at 0.8 Pa, and then magnetron sputtering a Cr target (with a purity higher than 99.95%) to deposit CrN on the surface of the Cr layer, the distance between the 2Cr13 martensitic stainless steel substrate and the Cr target was 60 cm, the Cr target current was 3.0 A, and a CrN layer (with a thickness of 0.2 μm) was formed;

[0049] 3) maintaining the argon flow rate, stopping the nitrogen flow, maintaining the working gas pressure at 0.5 Pa, and under the condition that the 2Cr13 martensitic stainless steel substrate is at room temperature (25°C), magnetron sputtering graphite target, B4C target (purity higher than 99.5%, B content of 85%) and WC target (purity higher than 99.5%, W content of 95%) are used to deposit DLC, B4C and WC on the surface of the CrN layer, with an average sputtering power of 5.0 kW and a bias voltage of -250 V, to form a DLC-B4C-WC composite layer (thickness of 0.3 μm);

[0050] 4) maintaining the argon flow rate and the working gas pressure at 0.5 Pa, and under the condition that the 2Cr13 martensitic stainless steel substrate is at room temperature (25°C), magnetron sputtering graphite target and MoS2 target are used to deposit DLC and MoS2 on the surface of the DLC-B4C-WC composite layer, with an average sputtering power of 3.0 kW and a bias voltage of -250 V, to form a DLC-MoS2 composite layer (with a thickness of 0.3 μm);

[0051] 5) Repeat the operations of step 3) and step 4) to alternately deposit DLC-B4C-WC composite layers and DLC-MoS2 composite layers to form a functional layer consisting of 8 DLC-B4C-WC composite layers and 8 DLC-MoS2 composite layers alternating with each other, turn off the power supply and bias, turn off the gas, and take out the 2Cr13 martensitic stainless steel substrate after it cools to room temperature, thereby obtaining a wear-resistant and self-lubricating diamond-like composite coating.

[0052] Performance Test:

[0053] 1) The surface hardness of the wear-resistant self-lubricating diamond-like composite coating of this embodiment was tested using a NANO G200 nanoindentation measuring instrument. The test showed that the surface hardness of the wear-resistant self-lubricating diamond-like composite coating was as high as 20.6 GPa.

[0054] 2) The tribological properties of the wear-resistant self-lubricating diamond-like carbon-based composite coating of this embodiment were tested under vacuum and room temperature using a HVTRB CSM friction tester. The obtained friction coefficient-friction cycle number relationship curve is shown in FIG. Figure 2 shown.

[0055] Depend on Figure 2 It can be seen that the average friction coefficient of the wear-resistant and self-lubricating diamond-like carbon-based composite coating in a vacuum environment is as low as 0.019, and the average wear rate is as low as 2.52×10 -7 m 3 / N·m, and it has not failed after 12,000 friction cycles. It has excellent self-lubricating effect and long service life.

[0056] Embodiment 2:

[0057] A wear-resistant and self-lubricating diamond-like carbon-based composite coating is prepared in the same manner as in Example 1 except that the average sputtering power in step 3) is adjusted from 5.0 kW to 6.0 kW.

[0058] After testing (the testing method is the same as that of Example 1), the surface hardness of the wear-resistant self-lubricating diamond-like carbon-based composite coating of this embodiment is as high as 18.3 GPa, the average friction coefficient is as low as 0.017 under vacuum and room temperature, and the average wear rate is as low as 1.99×10 -7 m 3 / N·m, and the friction cycle times exceed 12,000 times without failure, with excellent self-lubricating effect and long service life.

[0059] Embodiment 3:

[0060] A wear-resistant self-lubricating diamond-like carbon-based composite coating is prepared in the same manner as in Example 1 except that the bias voltage in step 3) and step 4) is adjusted from -250V to -150V.

[0061] After testing (the testing method is the same as that of Example 1), the surface hardness of the wear-resistant self-lubricating diamond-like composite coating of this embodiment is as high as 19.8 GPa, the average friction coefficient is as low as 0.019 under vacuum and room temperature, and the average wear rate is as low as 2.35×10 -7 m 3 / N·m, and the friction cycle times exceed 12,000 times without failure, with excellent self-lubricating effect and long service life.

[0062] Embodiment 4:

[0063] A wear-resistant and self-lubricating diamond-like composite coating is identical to the wear-resistant and self-lubricating diamond-like composite coating of Example 1, except that the thickness of the DLC-B4C-WC composite layer and the DLC-MoS2 composite layer are adjusted from 0.3 μm to 0.1 μm.

[0064] After testing (the testing method is the same as that of Example 1), the surface hardness of the wear-resistant self-lubricating diamond-like composite coating of this embodiment is as high as 18.4 GPa, the average friction coefficient is as low as 0.018 under vacuum and room temperature, and the average wear rate is as low as 2.10×10 -7 m 3 / N·m, and the friction cycle times exceed 12,000 times without failure, with excellent self-lubricating effect and long service life.

[0065] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A wear-resistant self-lubricating diamond-like carbon-based composite coating, characterized in that: The composition includes a Cr layer, a CrN layer and a functional layer which are stacked in sequence; the composition of the functional layer includes a plurality of DLC-B4C-WC composite layers and a plurality of DLC-MoS2 composite layers, and the DLC-B4C-WC composite layers and the DLC-MoS2 composite layers are alternately arranged; the layer closest to the CrN layer in the functional layer is the DLC-B4C-WC composite layer, and the layer farthest from the CrN layer is the DLC-MoS2 composite layer.

2. The wear-resistant self-lubricating diamond-like carbon-based composite coating according to claim 1, characterized in that: The thickness of the Cr layer is 0.1 μm to 0.2 μm; the thickness of the CrN layer is 0.1 μm to 0.2 μm.

3. The wear-resistant self-lubricating diamond-like carbon-based composite coating according to claim 1 or 2, characterized in that: The thickness of the functional layer is 1.5 μm to 5 μm; the thickness of the DLC-B4C-WC composite layer is 0.01 μm to 0.3 μm; and the thickness of the DLC-MoS2 composite layer is 0.01 μm to 0.3 μm.

4. A method for preparing a wear-resistant self-lubricating diamond-like carbon-based composite coating according to any one of claims 1 to 3, characterized in that: The following steps are involved: 1) In a protective atmosphere, Cr is deposited on the surface of a metal substrate by DC magnetron sputtering a Cr target to form a Cr layer; 2) In a protective atmosphere containing nitrogen, CrN is deposited on the surface of the Cr layer by DC magnetron sputtering of a Cr target to form a CrN layer; 3) In a protective atmosphere, DLC, B4C and WC are deposited on the surface of the CrN layer by high-power pulsed magnetron sputtering of graphite targets, B4C targets and WC targets to form a DLC-B4C-WC composite layer; 4) In a protective atmosphere, DLC and MoS2 are deposited on the surface of the DLC-B4C-WC composite layer by medium frequency magnetron sputtering of a graphite target and a MoS2 target to form a DLC-MoS2 composite layer; 5) Repeat the operations of step 3) and step 4) to alternately deposit DLC-B4C-WC composite layers and DLC-MoS2 composite layers to form a functional layer, thereby obtaining a wear-resistant and self-lubricating diamond-like carbon-based composite coating.

5. The preparation method according to claim 4, characterized in that: Step 1) The metal matrix is ​​one of a 2Cr13 martensitic stainless steel matrix, a 05Cr17Ni4Cu4Nb martensitic stainless steel matrix, and a YG6 cemented carbide matrix.

6. The preparation method according to claim 4 or 5, characterized in that: Step 1) The DC magnetron sputtering is carried out under the conditions of a working gas pressure of 0.4Pa to 1.0Pa and a Cr target current of 1.0A to 3.0A.

7. The preparation method according to claim 4 or 5, characterized in that: Step 2) The DC magnetron sputtering is carried out under the conditions of a working gas pressure of 0.8Pa to 1.0Pa and a Cr target current of 1.0A to 3.0A.

8. The preparation method according to claim 4 or 5, characterized in that: Step 3) The high-power pulsed magnetron sputtering is carried out under the conditions of a working gas pressure of 0.5Pa to 1.0Pa, an average sputtering power of 2.0kW to 6.0kW, and a bias voltage of -350V to 0V.

9. The preparation method according to claim 4 or 5, characterized in that: Step 4) The medium frequency magnetron sputtering is carried out under the conditions of a working gas pressure of 0.5Pa to 1.0Pa, an average sputtering power of 0.5kW to 3.0kW, and a bias voltage of -350V to 0V.

10. An aerospace equipment, characterized in that: A wear-resistant, self-lubricating diamond-like carbon-based composite coating comprising any one of claims 1 to 3.

Citation Information

Patent Citations

  • Hard high-temperature resistant self-lubricating coating product and preparation method thereof

    CN105584148A

  • Compound diamond carbon film and preparation method thereof

    CN107034440A

  • MoS2 / GIC (graphite intercalation compound) multi-layer composite solid lubrication coating used for aerospace hot working separation and preparation method

    CN108950550A

  • Gradient self-lubricating composite coating and preparation method thereof

    CN113621912A

  • Process method for enhancing bonding strength, corrosion resistance and wear resistance of diamond-like carbon coating