Novel organic-inorganic hybrid copper-based perovskite scintillation crystal and preparation method thereof

By preparing organic and inorganic hybrid copper-based perovskite scintillation crystals by using chemical solution precipitation method in an acidic environment, the environmental pollution and stability problems of lead-based perovskite materials are solved, and a high-yield, green and environmentally friendly scintillation crystal preparation is achieved. , suitable for LED and X-ray imaging and other fields.

CN118932486APending Publication Date: 2024-11-12SHANGHAI INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410936900.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing lead-based perovskite materials have problems such as heavy metal lead pollution to the human body and the environment, high environmental requirements, low yields, and production of harmful chemicals, and their self-absorbing effects and stability are poor, which limits their application.

Method used

A novel organic and inorganic hybrid copper-based perovskite scintillation crystal is prepared by using chemical solution precipitation method under acidic environment, with zero-dimensional perovskite structure, and the chemical formula is A2Cu2X6, X includes halogen elements such as Cl, Br, and I. , high yield scintillation crystals are obtained through a simple preparation process, and the production of harmful chemicals is avoided.

Benefits of technology

It realizes scintillation crystals with high spectral regulation, simple preparation process, short cycle, green and environmentally friendly and low cost, improves the stability and photoluminescence efficiency of the material, is suitable for large-scale production, and solves the environmental pollution problem of lead-based materials. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932486A_ABST
    Figure CN118932486A_ABST
Patent Text Reader

Abstract

The invention relates to the field of photoelectric device materials, in particular to a novel organic-inorganic hybrid copper-based perovskite scintillation crystal and a preparation method thereof.Cuprous oxide and organic molecules are dissolved in a hydrogen halide and hypophosphorous acid mixed solution, and the novel organic-inorganic hybrid copper-based perovskite scintillation crystal grows through a saturated recrystallization method. The crystal has excellent optical performance and scintillation performance, and is suitable for the fields of LED illumination, radiation detection, medical imaging and the like. Compared with the prior art, the problems that the heavy metal lead element of a lead-based perovskite material in the prior art is harmful to human bodies and pollutes the environment, the requirement for the preparation environment is high, the yield is low, and chemical substances harmful to the environment are generated in the preparation process can be solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of optoelectronic device materials, and in particular relates to a novel organic-inorganic hybrid copper-based perovskite scintillating crystal and a preparation method and application thereof. Background Art

[0002] In the past few decades, scintillator and radiation detection technology have made rapid progress, promoting the development of various high-performance commercial scintillating materials, such as CsI:Tl, LaBr3:Ce, CdWO4, Bi4Ge3O 12 (BGO), etc. However, the preparation process of these traditional scintillator materials is complicated, usually requiring high vacuum conditions and high synthesis temperature, and the cost is high. In addition, with the continuous upgrading of technology, the requirements for scintillator performance are also higher. Lead-based halide perovskite materials such as CsPbBr3 nanocrystals are regarded as candidate materials for the next generation of X-ray scintillators due to their advantages such as high absorption coefficient, high photoluminescence quantum yield (PLQYs), and tunable radioluminescence (RL) wavelength. However, lead-based halide perovskites have serious self-absorption effects, poor stability, and lead toxicity, which limit their further practical applications. Therefore, lead-free metal halide scintillators have become the focus of research, including double perovskites, copper, tin, manganese and other metal halides. Compared with double perovskites and silver-based scintillators, copper-based halide scintillators have good air stability, large X-ray attenuation efficiency, high light yield and other advantages, and are considered to be a very promising class of X-ray scintillating materials. In this regard, organic-inorganic hybrid metal halides contain a large number of organic cations in the lattice, which are looser and softer than all-inorganic systems, and have stronger exciton-phonon coupling, which is conducive to enhancing the emission of self-trapped excitons and showing excellent luminescence properties. However, the research reports on its scintillation properties are relatively scattered and scarce, and further in-depth exploration is needed.

[0003] In summary, the research and development of lead-free metal halide scintillators is of great significance to promoting the development of scintillators and radiation detection technology, while organic-inorganic hybrid copper-based metal halide materials show potential advantages and are worthy of in-depth research and exploration. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide an organic-inorganic hybrid copper-based perovskite scintillating crystal with the characteristics of high spectral controllability, simple preparation process, short cycle, high yield, green environmental protection and low cost, so as to solve the problems of heavy metal lead element in lead-based perovskite materials in the prior art that is harmful to the human body and pollutes the environment, has high requirements for the preparation environment, low yield, and produces chemical substances harmful to the environment during the preparation process; further provide a chemical solution precipitation method in an acidic environment to prepare the novel organic-inorganic hybrid copper-based perovskite scintillating crystal, so as to achieve the purposes of high yield, simple preparation process, short cycle, no output of harmful chemical substances, and suitability for large-scale production.

[0005] To achieve the above objectives, the present invention designs a novel organic-inorganic hybrid copper-based perovskite scintillating crystal. The crystal structure of the material belongs to zero-dimensional perovskite, and the general chemical formula is: A2Cu2X6, wherein A is a cation containing two ammonium ions, and X is a halogen element, and X includes one or a combination of Cl, Br, and I.

[0006] Further, when X represents Br, the material belongs to the monoclinic system and the P21 / c space group; in the crystal structure of the material, each Cu atom is connected by 4 Br atoms, and adjacent Cu atoms share two Br atoms, so adjacent tetrahedrons are connected together in a collinear form to form a unit [Cu2Br6] 4- Corner-sharing tetrahedral dimer cluster structure. [Cu2Br6] 4- The corner-sharing tetrahedral dimers are surrounded by A cations and isolated from each other, forming a typical zero-dimensional 0D structure at the molecular level.

[0007] Furthermore, the emission peak wavelength of the organic-inorganic hybrid copper-based perovskite scintillating crystal is in the range of 400 to 700 nm, and the photoluminescence efficiency PLQY is 98.11%.

[0008] The method for preparing the organic-inorganic hybrid copper-based perovskite scintillating crystal comprises the following steps:

[0009] Step S1, mixing cuprous oxide powder with HX solution, stirring with a magnetic stirrer for 5 to 8 minutes until completely dissolved, to obtain solution 1;

[0010] Step S2, mixing solution 1 with a hypophosphorous acid solution, stirring with a magnetic stirrer for 3 to 5 minutes, and mixing evenly to obtain solution 2; the hypophosphorous acid is a hypophosphorous acid aqueous solution with a mass fraction of 50%, and the volume ratio of solution 1 to the hypophosphorous acid solution is 1:2.5 to 4.5;

[0011] Step S3, mixing A with the heated solution 2, heating to ≥70°C and continuously heating with magnetic stirring for ≥20 min, and obtaining solution 3 after sufficient reaction; the heating temperature is ≥70°C and <95°C, and the molar mass ratio of cuprous oxide to A is 0.7:1-2;

[0012] Step S4, cooling the solution 3 in an air environment and standing for 8 hours to grow crystals;

[0013] Step S5, washing, filtering and drying the crystals obtained in step S4 to obtain the novel organic-inorganic hybrid copper-based perovskite scintillating crystals.

[0014] Furthermore, the cuprous oxide in step S1 has a purity of 99%, and the molar ratio of cuprous oxide powder to HX solution is 1:23-32.

[0015] Furthermore, in step S2, the hypophosphorous acid is a hypophosphorous acid aqueous solution with a mass fraction of 50%, and the volume ratio of solution 1 to the hypophosphorous acid solution is 1:2.5-4.5.

[0016] Furthermore, in step S3, the heating temperature is ≧70° C. and <95° C., and the molar mass ratio of cuprous oxide to A is 0.7:1-2.

[0017] Furthermore, in step (5), the washing solvent is any one of acetone, ether, ethyl acetate or methyl acetate.

[0018] The organic-inorganic hybrid copper-based perovskite scintillation crystal material is applied to green light LED, white light LED, flexible light-emitting film or scintillator imaging.

[0019] Compared with the prior art, the present invention has the characteristics of high spectral controllability, simple preparation process, short cycle, high yield, green environmental protection and low cost. It can solve the problems in the prior art that heavy metal lead elements in lead-based perovskite materials are harmful to the human body and pollute the environment, have high requirements for the preparation environment, low yield, and produce environmentally harmful chemicals in the preparation process.

[0020] Compared with the prior art, the present invention has the following advantages:

[0021] The present invention provides a novel organic-inorganic hybrid copper-based perovskite scintillation crystal, in which the organic cation at position A is [Cu2Br6] 4- Corner-sharing tetrahedral dimer structures separate to form a zero-dimensional structure.

[0022] The novel organic-inorganic hybrid copper-based perovskite scintillating crystal obtained by the present invention has the characteristics of being green and environmentally friendly, and can solve the problem faced by the perovskite in the prior art that it is rich in heavy metal lead elements that are difficult to degrade after multiple cycles;

[0023] The present invention provides a novel organic-inorganic hybrid copper-based perovskite scintillating crystal and a preparation method thereof. In the preparation method, the crystal material has a high yield, high spectrum controllability, excellent material luminescence performance, a wide emission spectrum coverage range, and a high luminescence efficiency of 98.11%.

[0024] The present invention provides a novel organic-inorganic hybrid copper-based perovskite scintillating crystal and a preparation method thereof. In the preparation method, the organic-inorganic hybrid copper-based perovskite scintillating crystal is prepared by a saturated recrystallization method in an acidic environment to protect the Cu + The advantages of not being oxidized and improving stability provide a new strategy for improving the stability of perovskite materials;

[0025] It has high market value and can be widely used in green LED, yellow LED, white LED or flexible light-emitting film and X-ray imaging and other fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a schematic diagram of the preparation process in Example 1 of the present invention.

[0027] Figure 2 This is an optical photograph of the novel organic-inorganic hybrid copper-based perovskite scintillating crystal prepared in Example 1 of the present invention.

[0028] Figure 3 This is a photoluminescence image of the novel organic-inorganic hybrid copper-based perovskite scintillating crystal prepared in Example 1 of the present invention.

[0029] Figure 4 This is a fluorescence quantum efficiency diagram of the new organic-inorganic hybrid copper-based perovskite scintillating crystal prepared in Example 1 of the present invention.

[0030] Figure 5 This is the XRD diffraction pattern of the novel organic-inorganic hybrid copper-based perovskite scintillating crystal powder prepared in Example 1 of the present invention measured under a standard XRD light source.

[0031] Figure 6 This is a diagram of the structure of the novel organic-inorganic hybrid copper-based perovskite scintillating crystal prepared in Example 1 of the present invention.

[0032] Figure 7 This is a SEM image of the novel organic-inorganic hybrid copper-based perovskite scintillating crystal prepared in Example 1 of the present invention.

[0033] Figure 8 This is an X-ray spectrum of the novel organic-inorganic hybrid copper-based perovskite scintillating crystal prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0034] In order to better understand the purpose, technical solutions and advantages of the present invention, the above technical solutions will be described in detail below in conjunction with the accompanying drawings and specific implementation methods. The specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention. In addition, the technical features involved in the following embodiments of the present invention can be combined with each other if they do not conflict with each other.

[0035] Example 1

[0036] Table 1. Amount of each reagent in Example 1

[0037]

[0038]

[0039] according to Figure 1 , perform the following preparation steps according to the amounts of each reagent shown in Table 1:

[0040] Step S1, weigh 0.15 g of Cu2O (1.8 mmol) and put it into a 25 ml beaker, add a magnet, use a pipette to measure 4.5 ml of HBr solution and add it to the beaker containing Cu2O, stir at a rate of 500 rpm, and stir at room temperature for 3 to 5 minutes until the Cu2O is completely dissolved to obtain solution 1.

[0041] Step S2, using a pipette to drop 13 ml of hypophosphorous acid solution into the solution 1 obtained in step S1, heating and stirring at room temperature for 3 to 5 minutes, the solution becomes clear and transparent, and a solution 2 is obtained.

[0042] Step S3, heat the solution obtained in step S2 to 50°C, weigh the corresponding amount of ODA in Table 1, continue heating to 90°C, and heat at a constant temperature for 20 minutes.

[0043] Step S4, when the time is up, stop heating, and let the resulting solution stand and cool to room temperature for 8 hours to grow crystals.

[0044] Step S5, washing, filtering and drying the obtained crystals to obtain the novel organic-inorganic hybrid copper-based perovskite scintillating crystals.

[0045] according to Figure 2 It can be seen that the optical photograph of the organic-inorganic hybrid copper-based perovskite scintillating crystal prepared by No. 5 in Example 1. Figure 2 It can be seen that (C8H 22 N2)2Cu2Br6 crystals emit green fluorescence.

[0046] according to Figure 3 It can be seen from the photoluminescence image of the organic-inorganic hybrid copper-based perovskite scintillating crystal powder prepared by No. 5 in Example 1 that the emission peak is located at 515nm, in the green light region.

[0047] according to Figure 4 It can be seen that the organic-inorganic hybrid copper-based perovskite scintillating crystal powder prepared in Example 1, No. 5, has a photoluminescence quantum yield of up to 98.11%.

[0048] according to Figure 5 It can be seen from the X-ray diffraction (PXRD) pattern of the organic-inorganic hybrid copper-based perovskite scintillating crystal powder prepared in Example 1, No. 5, that the diffraction peak is narrow and high, indicating that the sample is perfectly crystallized, the grains are large, and it shows high crystal quality.

[0049] according to Figure 6 It can be seen that the single crystal analytical structure of the organic-inorganic hybrid copper-based perovskite scintillating crystal prepared in Example 1, No. 5. The obtained crystal belongs to the monoclinic system and the P21 / c space group; in the crystal structure of the material, each Cu atom is connected by 4 Br atoms, and adjacent Cu atoms share two Br atoms, so adjacent tetrahedrons are connected together in a collinear form to form a unit [Cu2Br6] 4- Corner-sharing tetrahedral dimer cluster structure. [Cu2Br6] 4- Corner-sharing tetrahedral dimers are (C8H 22 N2) 2+ The cations are surrounded and isolated from each other, forming a typical zero-dimensional 0D structure at the molecular level.

[0050] according to Figure 7 It can be seen from the scanning electron microscope (SEM) image of the organic-inorganic hybrid copper-based perovskite scintillating crystal prepared in Example 1, No. 5, that the crystal is flaky, which is consistent with the macroscopic appearance.

[0051] according to Figure 8 It can be seen that the X-ray spectrum of the organic-inorganic hybrid copper-based perovskite scintillating crystal prepared by No. 5 in Example 1 shows that the crystal can be used in the field of scintillation.

[0052] Example 2

[0053] Table 2, the amount of each reagent in Example 2

[0054]

[0055] according to Figure 1 , perform the following preparation steps according to the amounts of each reagent shown in Table 2:

[0056] Step S1, weigh the corresponding amount of Cu2O / CuO in Table 1 and put it into a 25 ml beaker, add a magnet, use a pipette to measure the corresponding amount of HBr solution in Table 1 and add it to the beaker containing Cu2O / CuO, stir at a rate of 500 rpm, and stir at room temperature for 3 to 5 minutes until Cu2O is completely dissolved to obtain Solution 1.

[0057] Step S2, using a pipette to add 13 ml of hypophosphorous acid solution to the solution 1 obtained in step S1, stirring at room temperature for 3 to 5 minutes, the solution becomes clear and transparent, and a solution 2 is obtained.

[0058] Step S3, heating the solution obtained in step S2 to 50°C, weighing 1.5 mmol ODA, and continuing to heat to 90°C, and heating at a constant temperature for 20 minutes.

[0059] Step S4, when the time is up, stop heating, and let the resulting solution stand and cool to room temperature for 8 hours to grow crystals.

[0060] Step S5, washing, filtering and drying the obtained crystals to obtain the novel organic-inorganic hybrid copper-based perovskite scintillating crystals.

[0061] According to the control variable method as shown in Table 2, the Cu + , Cu 2+ Organic-inorganic hybrid copper-based perovskite scintillating crystal Cu + The luminous intensity is stronger.

[0062] Example 3

[0063] Table 3, the amount of each reagent in Example 3

[0064]

[0065] according to Figure 1 , perform the following preparation steps according to the amounts of each reagent shown in Table 3:

[0066] Step S1, weigh 1 mmol of Cu2O and put it into a 25 ml beaker, add a magnet, use a pipette to measure the corresponding amount of HCl / HBr / HI solution in Table 1 and add it to the beaker containing Cu2O, stir at a rate of 500 rpm, and stir at room temperature for 3 to 5 minutes until the Cu2O is completely dissolved to obtain Solution 1.

[0067] Step S2, using a pipette to add 13 ml of hypophosphorous acid solution to the solution 1 obtained in step S1, stirring at room temperature for 3 to 5 minutes, the solution becomes clear and transparent, and a solution 2 is obtained.

[0068] Step S3, heating the solution obtained in step S2 to 50°C, weighing 1.5 mmol ODA, and continuing to heat to 90°C, and heating at a constant temperature for 20 minutes.

[0069] Step S4, when the time is up, stop heating, and let the resulting solution stand and cool to room temperature for 8 hours to grow crystals.

[0070] Step S5, washing, filtering and drying the obtained crystals to obtain the novel organic-inorganic hybrid copper-based perovskite scintillating crystals.

[0071] According to Example 3, it can be seen that the emission peak of the spectrum shifts with the change of X, Cl red-shifts, and I blue-shifts, indicating that the spectrum of the organic-inorganic hybrid copper-based perovskite scintillating crystal can be regulated by the preparation method.

[0072] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A new type of organic-inorganic hybrid copper-based perovskite scintillating crystal, Features: The material crystal structure belongs to zero-dimensional perovskite, and the general chemical formula is: A 2 Cu 2 X 6 , wherein A is a cation containing two ammonium ions, X is a halogen element, and X includes one or a combination of Cl, Br, and I.

2. A novel organic-inorganic hybrid copper-based perovskite scintillating crystal as claimed in claim 1, It is characterized in that The A is C 8 H 20 N 2 , C 2 H 8 N 2 , C 3 H 10 N 2 , C 4 H 12 N 2 , C 7 H 18 N 2 , C 6 H 16 N 2 .

3. A novel organic-inorganic hybrid copper-based perovskite scintillating crystal as claimed in claim 1, It is characterized in that When X represents Br, [Cu 2 Br 6 ] 4- Zero-dimensional 0D structure of corner-sharing tetrahedral dimer clusters.

4. The method for preparing the organic-inorganic hybrid copper-based perovskite scintillating crystal according to any one of claims 1 to 3, It is characterized in that The steps include: Step S1, mixing cuprous oxide powder with HX solution, stirring with a magnetic stirrer for 5 to 8 minutes until completely dissolved, to obtain solution 1; Step S2, mixing solution 1 with a hypophosphorous acid solution, stirring with a magnetic stirrer for 3 to 5 minutes, and mixing evenly to obtain solution 2; Step S3, mixing A with the heated solution 2, heating to ≥70°C and continuously heating with magnetic stirring for ≥20 min, and obtaining solution 3 after sufficient reaction; Step S4, cooling the solution 3 at room temperature and standing for 8 hours to grow crystals; Step S5, washing, filtering and drying the crystals obtained in step (4) to obtain the novel organic-inorganic hybrid copper-based perovskite scintillating crystals.

5. The method for preparing an organic-inorganic hybrid copper-based perovskite scintillating crystal according to claim 4, wherein the cuprous oxide in step S1 has a purity of 99%, and the molar ratio of cuprous oxide powder to HX solution is 1:23-32.

6. The method for preparing the organic-inorganic hybrid copper-based perovskite scintillating crystal according to claim 4, It is characterized in that In step S2, the hypophosphorous acid is a hypophosphorous acid aqueous solution with a mass fraction of 50%, and the volume ratio of solution 1 to the hypophosphorous acid solution is 1:2.5-4.

5.

7. The method for preparing the organic-inorganic hybrid copper-based perovskite scintillating crystal according to claim 4, It is characterized in that The heating temperature in step S3 is ≧70° C. and <95° C., and the molar mass ratio of cuprous oxide to A is 0.7:1-2.

8. The method for preparing the organic-inorganic hybrid copper-based perovskite scintillating crystal according to claim 4, It is characterized in that In step (5), the washing solvent is any one of acetone, ether, ethyl acetate or methyl acetate.

9. Use of the organic-inorganic hybrid copper-based perovskite scintillating crystal according to any one of claims 1 to 3, It is characterized in that The 8 H 22 N 2 ) 2 Cu 2 X 6 Crystalline materials are used in green LEDs, white LEDs, flexible light-emitting films or X-ray imaging.