Method for preparing sizing carbon fiber by using polyester-containing polyurethane pre-sizing agent, application of sizing carbon fiber, sizing carbon fiber and application of sizing carbon fiber

By using pre-sizing agents of polyester polyurethane and epoxy resins and secondary sizing technology of resorcinol formaldehyde latex on carbon fibers, the problems of insufficient bonding power and poor wear resistance of carbon fibers and rubber materials are solved, and high efficiency is achieved The interface bonding and wear resistance are improved.

CN118932727APending Publication Date: 2024-11-12CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310536585.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The interface bonding between carbon fiber and rubber material is not strong and has poor wear resistance, which limits its application in high-strength friction conditions.

Method used

The carbon fiber is pre-sizing and pre-dryed with a pre-sizing agent containing polyester polyurethane and epoxy resin, followed by secondary sizing and drying with resorcinol formaldehyde latex to improve the adhesion between carbon fiber and rubber matrix and wear resistance. sex.

Benefits of technology

It significantly improves the wear resistance and adhesion of carbon fiber, enhances the interface bonding ability with the rubber matrix, and improves the temperature resistance, and is suitable for high-temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004226497990000111
    Figure BDA0004226497990000111
  • Figure BDA0004226497990000121
    Figure BDA0004226497990000121
  • Figure BDA0004226497990000122
    Figure BDA0004226497990000122
Patent Text Reader

Abstract

The invention relates to the field of carbon fiber sizing agents, in particular to a method for preparing sizing carbon fibers by using a polyester-containing polyurethane pre-sizing agent, application of the sizing carbon fibers, the sizing carbon fibers and application of the sizing carbon fibers. The method comprises the following steps: S1, carrying out pre-sizing and pre-drying on carbon fibers by adopting a pre-sizing agent containing polyester polyurethane and epoxy resin to obtain initial carbon fibers; s2, carrying out secondary sizing and secondary drying on the initial carbon fiber by adopting resorcinol formaldehyde latex to obtain sized carbon fiber; the infiltration time of the pre-sizing agent is less than or equal to 25 seconds, and the viscosity at 25 DEG C is less than or equal to 90 centipoises. Due to the existence of polyester polyurethane in the pre-sizing agent, the wear resistance of the carbon fibers can be remarkably improved, meanwhile, the bonding force between the sized carbon fibers and a rubber matrix is enhanced, and the temperature resistance of the sized carbon fibers is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of carbon fiber sizing agents, and in particular to a method for preparing sized carbon fibers by utilizing a polyester-containing polyurethane pre-sizing agent and application thereof, and the sized carbon fibers and applications thereof. Background Art

[0002] High-performance fiber-reinforced composites are one of the most promising new materials. Among them, carbon fiber-reinforced rubber composites can effectively combine the rigidity of carbon fiber and the flexibility of rubber. They have the advantages of high strength, high modulus, high elasticity, fatigue resistance and good dimensional stability, which expands the scope of use of rubber products and has a wide range of potential application value in applications with higher requirements such as tires, transmission belts, conveyor belts and high-pressure hoses. However, due to the performance differences between the two materials, there is a problem of weak interface bonding between carbon fiber and rubber materials. In carbon fiber reinforced resin composites, surface coating of water-based sizing agents is usually used to improve the problem of interface bonding, but there is no special sizing agent suitable for carbon fiber reinforced rubber materials. At the same time, many of the actual application occasions of carbon fiber reinforced rubber composites are long-term high-intensity friction conditions, so high requirements are also placed on the wear resistance of carbon fiber and carbon fiber reinforced rubber composites. There is no report on a special sizing agent that can simultaneously improve interface properties and wear resistance.

[0003] CN110983778A provides a sizing method for improving the wear resistance of carbon fiber, which uses a long drying process to improve the processing performance of carbon fiber, which is time-consuming, cannot be applied online, and cannot be applied to rubber substrates.

[0004] CN113355916A discloses a carbon fiber bundling agent, including acrylic modified polyurethane and vinyl ester resin. The prepared carbon fiber bundle has excellent wear resistance and process operability, and has good interface wettability and bonding strength with epoxy resin, but cannot improve the interface bonding ability with rubber matrix.

[0005] Therefore, how to overcome the above problems has become an important research topic in this field. Summary of the invention

[0006] The purpose of the present invention is to overcome the problem that the bonding force between sized carbon fiber and rubber matrix in the prior art is not strong, and the wear resistance is poor, resulting in limited subsequent applications. A method and application of preparing sized carbon fiber using a pre-sizing agent containing polyester polyurethane, sized carbon fiber and application are provided. The method is simple to operate. By coating a layer of pre-sizing agent containing polyester polyurethane and epoxy resin on the surface of carbon fiber and pre-drying, it can achieve initial bonding with the surface of carbon fiber, and then use resorcinol formaldehyde latex (hereinafter referred to as RFL emulsion) for secondary sizing and secondary drying. Since the pre-sizing agent has good hydrophilicity, the RFL emulsion can be quickly spread and infiltrated on the surface of carbon fiber coated with the pre-sizing agent, thereby improving the bonding force and bonding stability of carbon fiber and rubber matrix. At the same time, due to the presence of polyester polyurethane in the pre-sizing agent, the wear resistance of sized carbon fiber can be significantly improved, and the applicability of post-processing of sized carbon fiber can be improved.

[0007] In order to achieve the above object, the first aspect of the present invention provides a method for preparing sized carbon fiber using a polyester-containing polyurethane pre-sizing agent, the method comprising:

[0008] S1, pre-sizing and pre-drying the carbon fiber using a pre-sizing agent containing polyester polyurethane and epoxy resin to obtain initial carbon fiber;

[0009] S2, performing secondary sizing and secondary drying on the initial carbon fiber using resorcinol formaldehyde latex to obtain sizing carbon fiber;

[0010] The pre-sizing agent has a wetting time of ≤25 seconds and a viscosity of ≤90 centipoise at 25°C.

[0011] The second aspect of the present invention provides a sized carbon fiber prepared by the method for preparing sized carbon fiber using a polyester-containing polyurethane pre-sizing agent as described in the first aspect of the present invention.

[0012] The third aspect of the present invention provides a method for preparing sized carbon fibers using a polyester-containing polyurethane pre-sizing agent as described in the first aspect of the present invention, and use of the sized carbon fibers as described in the second aspect of the present invention in rubber materials.

[0013] Through the above technical scheme, the method and application of preparing sized carbon fiber containing polyester polyurethane pre-sizing agent, and the sized carbon fiber and application provided by the present invention achieve the following beneficial effects:

[0014] (1) The present invention uses epoxy resin and polyester polyurethane as the main components in the pre-sizing agent, and cooperates with a hydrophilic RFL emulsion sizing agent to significantly improve the wear resistance of the sized carbon fiber (the number of wear resistance times reaches more than 4900 times), and when the sized carbon fiber is applied to the rubber material, the bonding ability of the sized carbon fiber and the rubber matrix can be enhanced at the same time, and the bonding force can reach 130N or more;

[0015] (2) The present invention utilizes a pre-sizing agent and an RFL emulsion to perform pre-sizing and secondary sizing on carbon fibers, respectively, which can significantly improve the two-phase interface bonding ability between the prepared sized carbon fibers and the rubber matrix, while improving the temperature resistance of the sized carbon fibers, and can withstand high temperatures of above 250°C.

[0016] (3) The present invention controls the wetting time of the pre-sizing agent to be ≤25 seconds, the viscosity at 25°C to be ≤90 centipoise, and specific pre-sizing and secondary sizing processes, thereby ultimately preparing sized carbon fibers with excellent wear resistance, high temperature resistance, and good adhesion to the rubber matrix, thereby solving the technical problem of the interface performance between the sized carbon fibers and the rubber matrix.

[0017] (4) The method of the present invention is simple in process, highly stable, safe and pollution-free, and can be completed using an existing carbon fiber preparation production line, thus having broad industrial prospects. DETAILED DESCRIPTION

[0018] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0019] A first aspect of the present invention provides a method for preparing sized carbon fiber using a polyester-containing polyurethane pre-sizing agent, wherein the method comprises:

[0020] S1, pre-sizing and pre-drying the carbon fiber using a pre-sizing agent containing polyester polyurethane and epoxy resin to obtain initial carbon fiber;

[0021] S2, performing secondary sizing and secondary drying on the initial carbon fiber using resorcinol formaldehyde latex to obtain sizing carbon fiber;

[0022] The pre-sizing agent has a wetting time of ≤25 seconds and a viscosity of ≤90 centipoise at 25°C.

[0023] In the present invention, the inventors found that in the prior art, in order to improve the interface problem between carbon fiber and rubber matrix, RFL emulsion is often used to size carbon fiber. However, it is found in actual application that due to the weak bonding ability of RFL emulsion with the surface of carbon fiber, the bonding force between carbon fiber and rubber matrix after sizing cannot be effectively improved by using RFL emulsion alone. The inventors found through research that this is due to the poor wetting and spreading of RFL emulsion on the surface of carbon fiber, resulting in discontinuous and weak bonding points, and the obtained sized carbon fiber does not have good temperature resistance and wear resistance.

[0024] The inventors further discovered that by pre-coating a layer of pre-sizing agent containing polyester polyurethane and epoxy resin on the surface of carbon fiber and pre-drying it, and then performing secondary sizing with RFL emulsion and secondary drying, the RFL emulsion can be quickly spread and infiltrated on the surface of carbon fiber coated with the pre-sizing agent. Due to the presence of polyester polyurethane in the pre-sizing agent, the wear resistance of the sized carbon fiber can be significantly improved, and the temperature resistance of the sized carbon fiber can be improved at the same time. When the sized carbon fiber is used to reinforce rubber composite materials, the bonding force between the sized carbon fiber and the rubber matrix is ​​effectively improved.

[0025] The inventors further discovered that only when the infiltration time of the introduced pre-sizing agent is ≤25 seconds and the viscosity at 25°C is ≤90 centipoise, can it achieve good coordination with the RFL emulsion and provide a good coupling enhancement effect for the carbon fiber and the RFL emulsion. When the infiltration time is greater than 25 seconds, the hydrophilicity is insufficient, and the pre-sizing agent has insufficient binding ability with the carbon fiber and the RFL emulsion, and cannot play a role in coupling enhancement. When the viscosity is greater than 90 centipoise at 25°C, the expansion of the pre-sizing agent on the surface of the carbon fiber is greatly hindered, and it cannot be evenly infiltrated and spread, thereby greatly affecting the wear resistance of the carbon fiber and is not conducive to the improvement of the bonding force.

[0026] In the present invention, the epoxy resin is a glycidyl ether epoxy resin containing two or more epoxy groups in the molecule, for example, it may be at least one of bisphenol A, bisphenol F, and bisphenol S.

[0027] In the present invention, the epoxy equivalent of the epoxy resin is 160-6000.

[0028] In the present invention, the epoxy equivalent of the epoxy resin satisfies the above range, so that the wetting time and viscosity of the prepared pre-sizing agent at 25° C. can meet the requirements.

[0029] In the present invention, the pre-sizing agent may further contain components such as antioxidants, lubricants, surfactants, etc. The surfactant is preferably a non-ionic surfactant.

[0030] According to a preferred embodiment of the present invention, the nonionic surfactant is selected from at least one of alkylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether, fatty acid polyoxyethylene ester, polyoxyethylene amine, polyoxyethylene amide, sorbitan ester and fluorocarbon surfactant.

[0031] In the present invention, there is no particular limitation on the types and contents of the antioxidant, lubricant and surfactant contained in the pre-sizing agent, and they can be adjusted according to the needs in the art.

[0032] According to a particularly preferred embodiment of the present invention, the pre-sizing agent contains 35-55 parts of epoxy resin, 20-45 parts of polyester polyurethane, 1-5 parts of antioxidant, 1-5 parts of lubricant and 10-30 parts of surfactant. When each component meets the above range, the pre-sizing agent has a better effect when applied to sizing carbon fiber.

[0033] In the present invention, the epoxy resin, antioxidant, lubricant and surfactant may be provided in the form of an epoxy resin aqueous emulsion.

[0034] In the present invention, the epoxy resin, antioxidant, lubricant and surfactant are configured into an epoxy resin aqueous emulsion for addition, and further used in combination with the RFL emulsion, which can improve the synergistic effect between the components, significantly improve the wear resistance of the sized carbon fiber, improve the bonding force between the sized carbon fiber and the rubber matrix, and effectively improve the temperature resistance of the sized carbon fiber.

[0035] In the present invention, the preparation method of the pre-sizing agent in step S1 can adopt the preparation method of the emulsion generally used in the art, such as phase inversion emulsification method, ultrasonic emulsification method and colloid mill emulsification method.

[0036] In the present invention, the viscosity of the pre-sizing agent refers to the viscosity when the pre-sizing agent is diluted with water to a concentration of 2 wt %.

[0037] In the present invention, the RFL emulsion is a mixed emulsion formed by the reaction of resorcinol, formaldehyde and rubber emulsion. The specific preparation process is: sodium hydroxide and resorcinol are added to the first reaction kettle, and then an appropriate amount of water is added, the temperature is controlled to 20-40°C, and then formaldehyde is slowly added, and a prepolymer is obtained after aging reaction for 2-4 hours; rubber latex is added to the second reaction kettle, the temperature is controlled to 20-40°C, and the synthesized prepolymer is slowly added dropwise, and the reaction is continued for 10-30 hours to finally prepare the RFL emulsion.

[0038] In the present invention, the rubber emulsion in the RFL emulsion can be acrylic rubber emulsion, acrylonitrile-butadiene rubber emulsion, isoprene rubber emulsion, polyurethane rubber emulsion, ethylene-propylene rubber emulsion, chloroprene rubber emulsion, silicone rubber emulsion, hydrogenated nitrile rubber emulsion, styrene-butadiene rubber emulsion, polysulfide rubber emulsion, natural rubber emulsion, butadiene rubber emulsion and butyl rubber emulsion, etc.

[0039] According to the present invention, the pre-sizing agent has a wetting time of ≤10 seconds and a viscosity of ≤70 centipoise at 25°C.

[0040] According to the present invention, in the pre-sizing agent, the mass ratio of the epoxy resin to the polyester polyurethane is 1:0.5-0.9.

[0041] In the present invention, the mass ratio of the epoxy resin and the polyester polyurethane satisfies the above range, so that the wetting time and the viscosity of the pre-sizing agent at 25°C can meet the requirements, further improve the hydrophilicity and two-phase coupling of the pre-sizing agent, improve the bonding force between the sized carbon fiber and the rubber matrix, and at the same time, the sized carbon fiber has excellent wear resistance and good temperature resistance.

[0042] Furthermore, in the pre-sizing agent, the mass ratio of the epoxy resin to the polyester polyurethane is 1:0.6-0.8.

[0043] According to the present invention, the number average molecular weight of the polyester polyurethane is 3000-30000 g / mol, preferably 7000-15000 g / mol.

[0044] According to the present invention, the polyester polyurethane comprises a structural unit A provided by polyisocyanate and a structural unit B provided by polyester polyol.

[0045] Preferably, the molar ratio of the structural unit A to the structural unit B is 1-2:1;

[0046] Furthermore, the polyisocyanate is an aromatic polyisocyanate.

[0047] In the present invention, the polyisocyanate is selected from aromatic polyisocyanates, compared with aliphatic polyisocyanates, so that the prepared polyester polyurethane can further improve the wear resistance of sized carbon fibers when applied to the pre-sizing agent and used in combination with the RFL emulsion.

[0048] In the present invention, the aromatic polyisocyanate is selected from toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), naphthalene diisocyanate (NDI), p-phenylene diisocyanate (PPDI), polymethylene polyphenyl isocyanate (PAPI), etc., preferably at least one of toluene diisocyanate (TDI) and diphenylmethane diisocyanate (MDI).

[0049] In the present invention, the polyester polyol is not particularly limited, and may be, for example, polycaprolactone polyol and polycarbonate polyol, preferably an aromatic polyester polyol prepared by polycondensation of an aromatic dibasic acid and a diol.

[0050] In the present invention, the aromatic dibasic acid can be commercially available, for example, phthalic acid, isophthalic acid, and terephthalic acid.

[0051] In the present invention, the diol can be commercially available, for example, ethylene glycol, propylene glycol, or butylene glycol.

[0052] In the present invention, the polyester polyol can be obtained commercially.

[0053] According to the present invention, the pre-drying temperature is 70-110°C.

[0054] In the present invention, if the pre-drying temperature is too low (less than 70°C), the drying time will be too long and the dehydration efficiency will be low; if the pre-drying temperature is too high (greater than 110°C), the dehydration will be too fast and the moisture content will be difficult to control. The pre-dried fiber can retain appropriate moisture to promote the rapid spreading and penetration of the RFL emulsion.

[0055] Furthermore, the pre-drying temperature is 80-100°C.

[0056] According to the present invention, the temperature of the secondary drying is 100-250°C, preferably 150-200°C.

[0057] According to the present invention, in the resorcinol formaldehyde latex, the molar ratio of resorcinol to formaldehyde is 1:1-20, preferably 1:5-15.

[0058] According to the present invention, based on the mass of the carbon fiber, the pre-sizing amount of the pre-sizing agent is 0.1-30wt%.

[0059] In the present invention, if the pre-sizing amount of the pre-sizing agent is too small, the coupling effect of improving the interface cannot be achieved; if the pre-sizing amount is too large, the fiber bundling and fiber opening ability will be affected.

[0060] Furthermore, based on the mass of the carbon fiber, the pre-sizing amount of the pre-sizing agent is 0.5-20wt%.

[0061] According to the present invention, based on the mass of the carbon fiber, the sizing amount of the resorcinol formaldehyde latex is 5-35wt%.

[0062] In the present invention, when the sizing amount of the RFL emulsion is less than 5wt%, the adhesion between the sized carbon fiber and the rubber matrix is ​​insufficient; when it exceeds 35wt%, the post-processing of the sized fiber will be difficult and the fatigue resistance will be reduced.

[0063] Furthermore, based on the mass of the carbon fiber, the sizing amount of the RFL emulsion is 10-20wt%.

[0064] The second aspect of the present invention provides a sized carbon fiber prepared by the method for preparing sized carbon fiber using a polyester-containing polyurethane pre-sizing agent as described in the first aspect of the present invention.

[0065] The third aspect of the present invention provides a method for preparing sized carbon fibers using a polyester-containing polyurethane pre-sizing agent as described in the first aspect of the present invention, and use of the sized carbon fibers as described in the second aspect of the present invention in rubber materials.

[0066] In the present invention, when the sized carbon fiber is used in a rubber material to prepare a reinforced rubber composite material, the content of the sized carbon fiber in the reinforced rubber composite material is 15-30wt%.

[0067] In the present invention, the reinforced rubber composite material may further contain zinc oxide, stearic acid, carbon black N330, accelerator DM, accelerator TMTD and sulfur.

[0068] In the present invention, there is no particular limitation on the rubber material, and it may be, for example, acrylic rubber, acrylonitrile-butadiene rubber, isoprene rubber, polyurethane rubber, ethylene-propylene rubber, chloroprene rubber, silicone rubber, hydrogenated nitrile rubber, styrene-butadiene rubber, polysulfide rubber, natural rubber, butadiene rubber, or butyl rubber, and is preferably of the same type as the rubber emulsion in the RFL emulsion described in the present invention.

[0069] The present invention will be described in detail below through examples. In the following examples, each parameter is obtained by the following method.

[0070] Wetting time: The pre-sizing agent was evenly coated on the glass slide, placed at room temperature for 12 hours, and then dried at 50°C to obtain a film sample. Using the OCA20 high-speed contact angle meter, 3 microliters of deionized water was dropped onto the surface of the glass slide, and the time required for the water drop to completely wet the surface was recorded. Complete wetting was measured when the contact angle was 0.

[0071] Viscosity: The pre-sizing agent was diluted with water to a concentration of 2 wt %, and the viscosity was tested using a rotational viscometer at a temperature of 25° C. and a torque range of 30-70%.

[0072] Adhesion: The sizing carbon fiber is buried in an unvulcanized natural rubber block (wherein the mass of the sizing carbon fiber is 20% of the mass of the natural rubber block), and vulcanized at 140°C, 40 minutes, and a stamping pressure of 3MPa. The vulcanization formula system includes 100 parts of natural rubber, 4 parts of zinc oxide, 1.5 parts of stearic acid, 15 parts of carbon black N330, 1.2 parts of accelerator DM, 0.2 parts of accelerator TMTD, and 3 parts of sulfur. On a universal strength tester, the sizing carbon fiber is pulled out at a speed of 200mm / min. The tension required to pull out a length of 1 cm is the adhesion between the fiber and the rubber.

[0073] Sizing amount: Weigh the mass of carbon fiber before and after sizing, and calculate the sizing amount according to the formula: Sizing amount % = (mass of carbon fiber after sizing - mass of carbon fiber before sizing) / mass of carbon fiber before sizing × 100%.

[0074] Abrasion times: The TM200H yarn abrasion tester is used to test the number of times the sized carbon fiber is rubbed until it breaks.

[0075] Temperature resistance: Take an appropriate amount of sizing carbon fiber and test the weight loss rate in the range of room temperature-300°C using a TGA thermogravimetric analyzer under a nitrogen atmosphere (weight loss rate % = loss weight / sizing agent weight × 100%). The temperature corresponding to 5wt% weight loss rate is used as the temperature resistance index.

[0076] Polyester polyurethane was purchased from Shanghai Institute of Organic Chemistry, Chinese Academy of Sciences, with the brands Texin260, Texin345, Texin340X, Texin290, Texin180, and Texin245X;

[0077] KTM-2G epoxy emulsion sizing agent, purchased from Sinopharm Reagent;

[0078] SS-3 epoxy emulsion sizing agent was purchased from Sinopharm Reagent.

[0079] Examples 1-6

[0080] A quantitative epoxy resin, a surfactant, a polyester polyurethane, an antioxidant, and a lubricant are put into a reaction kettle, and an appropriate amount of deionized water is added, and a uniformly distributed stable emulsion is prepared by high-speed stirring and phase inversion emulsification, which is a pre-sizing agent. The components and amounts of the pre-sizing agent are shown in Table 1, and the infiltration time of the obtained pre-sizing agent is shown in Table 2.

[0081] Among them, the brands of epoxy resin are: E21, E51, E20, 6458, E44, 6445;

[0082] The surfactants are: polyethylene glycol PEG-4000, polyoxyethylene sorbitan fatty acid ester T-80, allyl polyethylene glycol APEG2000, fatty alcohol polyoxyethylene ether AEO-15, alkylphenol polyoxyethylene ether APEO-50, polypropylene glycol PPG-6000;

[0083] The lubricant is dioctyl phthalate DOP;

[0084] The brands of polyester polyurethane are: Texin260 (number average molecular weight is 11000), Texin345 (number average molecular weight is 7000), Texin340X (number average molecular weight is 1000), Texin290 (number average molecular weight is 12500), Texin180 (number average molecular weight is 25600), Texin245X (number average molecular weight is 9500).

[0085] In the first reactor equipped with a stirrer and a temperature control device, 10g of sodium hydroxide and a certain amount of resorcinol were added, and then 90g of water was added, stirred and heated to 35°C, and a certain amount of formaldehyde was slowly added, wherein the total amount of resorcinol and formaldehyde was 30g. After reacting for 3 hours, the temperature was slowly lowered to obtain a resin prepolymer; in the second reactor, 97g of natural rubber latex was added, stirred and heated to 35°C, and the synthesized resin prepolymer was slowly added dropwise, and the reaction continued for 20 hours, and the temperature was slowly lowered to obtain an RFL emulsion. The molar ratio of resorcinol to formaldehyde in the RFL emulsion is shown in Table 2.

[0086] The unsized carbon fiber is pre-sized in the first sizing tank filled with a certain viscosity diluent of the above-mentioned pre-sizing agent (the diluent is water, the specific viscosity is shown in Table 2), and then dried at a set drying temperature for 2 minutes; then it is secondary sized in the second sizing tank filled with a certain viscosity diluent of the above-mentioned RFL emulsion (the specific viscosity is shown in Table 2), and then dried at a set temperature for 3 minutes, and the sized carbon fiber for reinforcing rubber composite materials is prepared after winding and collecting. The pre-sizing amount and pre-drying temperature, the secondary sizing amount and the secondary drying temperature are shown in Table 2.

[0087] Comparative Example 1

[0088] The unsized carbon fiber was sized with commercially available KTM-2G epoxy emulsion sizing agent, the sizing amount was 5wt%, the drying temperature was 110°C, and the sized carbon fiber was prepared by winding and collecting.

[0089] Comparative Example 2

[0090] The unsized carbon fiber was sized using the RFL emulsion in Example 4, with a sizing amount of 10 wt % and a drying temperature of 160° C., to prepare the sized carbon fiber by winding and collecting.

[0091] Comparative Example 3

[0092] The unsized carbon fiber was pre-sized with a commercially available SS-3 epoxy emulsion sizing agent at a sizing amount of 5% and a drying temperature of 90°C to obtain initial carbon fiber; then the initial carbon fiber was secondary-sized with the RFL emulsion in Example 4 at a sizing amount of 10% and a drying temperature of 180°C, and the sized carbon fiber was prepared by winding and collecting.

[0093] Table 1

[0094]

[0095] Table 2

[0096]

[0097] Test Case

[0098] The sized carbon fibers prepared in the examples and comparative examples were tested for wear resistance, high temperature resistance and adhesion to the rubber matrix. The results are shown in Table 3.

[0099] Table 3

[0100]

[0101] From the results in the table, it can be seen that in Comparative Example 1, only the traditional epoxy resin emulsion is used, and in Comparative Example 2, only a single RFL emulsion is used, the bonding force between the prepared carbon fiber and the rubber matrix is ​​low, and the wear resistance is low. In Comparative Example 3, the complete impregnation time of the pre-sizing epoxy emulsion is too long, the viscosity is too high, and the improvement effect is not obvious.

[0102] In Examples 1-6, a pre-sizing agent with epoxy resin and polyester polyurethane resin emulsion as the main body, an impregnation time of ≤25 seconds and a viscosity of ≤90 centipoise is introduced in the pre-sizing process, and an RFL emulsion sizing agent with good affinity to the rubber matrix is ​​used in the secondary sizing process. The prepared sized carbon fibers have high temperature resistance, increased adhesion to the rubber matrix, and significantly improved wear resistance of the sized carbon fibers. At the same time, the technical problem of the interface performance between the sized carbon fibers and the rubber matrix is ​​solved.

[0103] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing sized carbon fiber using a polyester-containing polyurethane pre-sizing agent, characterized in that: The method comprises: S1, pre-sizing and pre-drying the carbon fiber using a pre-sizing agent containing polyester polyurethane and epoxy resin to obtain initial carbon fiber; S2, performing secondary sizing and secondary drying on the initial carbon fiber using resorcinol formaldehyde latex to obtain sizing carbon fiber; The pre-sizing agent has a wetting time of ≤25 seconds and a viscosity of ≤90 centipoise at 25°C.

2. The method according to claim 1, wherein: The pre-sizing agent has a wetting time of ≤10 seconds and a viscosity of ≤70 centipoise at 25°C.

3. The method according to claim 1 or 2, wherein: In the pre-sizing agent, the mass ratio of the epoxy resin to the polyester polyurethane is 1:0.5-0.9, preferably 1:0.6-0.

8.

4. The method according to claim 3, wherein: The number average molecular weight of the polyester polyurethane is 3000-30000 g / mol, preferably 7000-15000 g / mol.

5. The method according to any one of claims 1 to 4, wherein: The polyester polyurethane comprises a structural unit A provided by a polyisocyanate and a structural unit B provided by a polyester polyol; Preferably, the molar ratio of the structural unit A to the structural unit B is 1-2:1; Preferably, the polyisocyanate is an aromatic polyisocyanate.

6. The method according to any one of claims 1 to 5, wherein: The pre-drying temperature is 70-110°C, preferably 80-100°C; Preferably, the secondary drying temperature is 100-250°C, preferably 150-200°C.

7. The method according to any one of claims 1 to 6, wherein: In the resorcinol formaldehyde latex, the molar ratio of resorcinol to formaldehyde is 1:1-20, preferably 1:5-15.

8. The method according to any one of claims 1 to 7, wherein: Based on the mass of the carbon fiber, the pre-sizing amount of the pre-sizing agent is 0.1-30wt%, preferably 0.5-20wt%; Preferably, based on the mass of the carbon fiber, the sizing amount of the resorcinol formaldehyde latex is 5-35wt%, preferably 10-20wt%.

9. Sized carbon fiber prepared by the method for preparing sized carbon fiber using a polyester-containing polyurethane pre-sizing agent as described in any one of claims 1 to 8.

10. The method for preparing sized carbon fiber by using polyester-containing polyurethane pre-sizing agent as described in any one of claims 1 to 8, and the use of sized carbon fiber as described in claim 9 in rubber materials.

Citation Information

Cited By

  • Sizing method of graphene fiber

    CN121451436A