Composite film based on epoxy resin modification and preparation method thereof

By using epoxy resin modified composite film technology in OLED substrate materials, the problems of light transmittance and cost of existing OLED substrate materials are solved, and high light transmittance, low haze and good water vapor isolation performance are achieved. , improves the current density and power efficiency of OLED devices.

CN118932764APending Publication Date: 2024-11-12SHAANXI UNIV OF SCI & TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411023186.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing OLED substrate materials have shortcomings in light transmittance, cost, thermal stability and flexibility, which limits their long-term development in the fields of displays and consumer electronics.

Method used

Using the composite film preparation method based on epoxy resin modification, the high-beating cellulose film with high beating degree is immersed in the epoxy resin and double-sided coating treatment to prepare high light transmittance, low haze and good quality Composite film with water vapor isolation properties.

Benefits of technology

It improves the brightness, current density and power efficiency of OLED devices, reduces the preparation cost, meets the light transmittance and fold resistance requirements of OLED substrates, and improves the chemical stability of hydration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932764A_ABST
    Figure CN118932764A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a composite film based on epoxy resin modification. The preparation method specifically comprises the following steps: step 1, preparing a cellulose film; 2, preparing epoxy resin slurry; and 3, putting the cellulose film prepared in the step 1 into the epoxy resin slurry prepared in the step 2, completely dipping, and curing in a constant-temperature box to form a film, so as to obtain the cellulose / epoxy resin composite film. The invention also discloses a composite film based on epoxy resin modification. The composite film prepared by the invention has the characteristics of low cost, high light transmittance and long service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nanocellulose preparation and application, and relates to a composite film based on epoxy resin modification. The invention also relates to a preparation method of the composite film based on epoxy resin modification. Background Art

[0002] In recent years, with the rapid development of the domestic economy, OLED (organic light-emitting diode) has great advantages and potential in the display industry and consumer electronics. It has the characteristics of light weight, wide viewing angle, self-luminescence, high contrast and low energy consumption, and is widely used in TVs, mobile phones and tablets. Among them, the substrate, which plays a supporting role, has various effects on the optoelectronic properties of OLED devices. The substrate is widely used in OLED devices because of its advantages of high light transmittance, mechanical properties, thermal stability, flexibility and very low surface roughness.

[0003] However, the substrates currently used are mainly divided into three types, plastic substrates, glass substrates, metal foils, etc., but there are still some disadvantages. Although plastic substrates have high light transmittance, they have the disadvantages of low water and oxygen isolation, low processing temperature, and large thermal expansion coefficient; glass substrates have poor toughness and are prone to cracks after repeated bending; metal foils can achieve many indicators of flexible OLED substrates, but their light transmittance is very low and the preparation cost is high. These disadvantages limit the long-term development of existing substrate technology in the OLED field. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a composite film based on epoxy resin modification. The composite film prepared by the method has the characteristics of low cost, high light transmittance and long service life.

[0005] Another object of the present invention is to provide a composite film based on epoxy resin modification.

[0006] The first technical solution adopted by the present invention is a method for preparing a composite film based on epoxy resin modification, which specifically comprises the following steps:

[0007] Step 1, preparing a cellulose film;

[0008] Step 2, preparing epoxy resin slurry;

[0009] Step 3, completely immersing the cellulose film prepared in step 1 into the epoxy resin slurry prepared in step 2, and curing the cellulose film in a constant temperature box to form a film, thereby obtaining a cellulose / epoxy resin composite film.

[0010] The first technical solution of the present invention is also characterized in that:

[0011] The specific process of step 1 is:

[0012] Step 1.1, taking 30 g of absolutely dry hardwood as raw material fiber, preparing cellulose pulp with a beating degree of 70°SR to 90°SR;

[0013] Step 1.2: Set the weight of the cellulose film to 40.0 g / m 2 The cellulose slurry obtained in step 1.1 is subjected to a vacuum filtration process to prepare a wet cellulose film, which is then subjected to vacuum drying to obtain a dried cellulose film. The cellulose film is placed in a sealed bag and stored at room temperature for later use.

[0014] In step 1.1, the cellulose content in the hardwood is 40% to 50%.

[0015] In step 1.2, the vacuum drying temperature is 85° C. to 95° C., and the vacuum drying time is 4 min to 6 min.

[0016] The specific process of step 2 is:

[0017] Pour E51 epoxy resin into a disposable culture dish and heat it to 35°C, add 1,8-diamino-3,6-dioxaoctane curing agent into the disposable culture dish, put a magnetic bar into the disposable culture dish for magnetic stirring, and then transfer the disposable culture dish to a vacuum drying oven for degassing to obtain epoxy resin slurry.

[0018] In step 2, the rotation speed of the magnetic stirring is 90 rpm to 110 rpm, and the time of the magnetic stirring is 3 min to 5 min.

[0019] In step 2, the drying temperature in the vacuum drying oven is 50° C. to 70° C., and the vacuum drying time is 5 min to 7 min.

[0020] In step 2, the mass ratio of E51 epoxy resin to 1,8-diamino-3,6-dioxaoctane curing agent is 9:1.

[0021] The specific process of step 3 is: completely immerse the cellulose film prepared in step 1 in the epoxy resin prepared in step 2, then lift the immersed cellulose film with tweezers and hang it vertically in a constant temperature box for curing, and obtain a cellulose / epoxy resin composite film after curing.

[0022] The second technical solution adopted by the present invention is that the composite film based on epoxy resin modification is prepared by adopting the preparation method of the composite film based on epoxy resin modification.

[0023] The beneficial effects of the present invention are as follows:

[0024] 1. The present invention uses hardwood to prepare pulp, which can improve production efficiency; the produced paper has high bulk and stiffness, and improves paper quality. The present invention uses environmentally friendly, renewable and degradable hardwood fiber raw materials to prepare a high-transmittance, low-haze composite film.

[0025] 2. Compared with traditional PET (polyethylene terephthalate), the present invention selects a technology of preparing a composite film by impregnating a 90° SR cellulose film in an epoxy resin. The prepared composite film has improved brightness and current density of OLED light-emitting devices, and the current efficiency and power efficiency are close to those of PET, and the transmittance meets the OLED substrate indicators. In addition, the water vapor permeability of the films coated with single / double sides of epoxy resin is compared using a water vapor permeability meter, and it is found that the water vapor barrier performance of the film coated with a single layer of epoxy resin fails to meet the OLED technical indicators. Finally, it is found that the double-sided coating process of epoxy resin is more suitable for preparing OLED substrates.

[0026] 3. The strain of the high-beatenness cellulose film coated on both sides with epoxy resin in the present invention is higher than that of the uncoated film, reaching 2.7%, which is lower than the stress and strain of different commercial OLED substrates; the folding endurance of the high-beatenness cellulose film coated on both sides with epoxy resin is lower than the folding endurance of the OLED substrate. After the epoxy resin coating process, the cellulose film has good hydration chemical stability; at the same time, its surface is hydrophilic, which promotes the deposition of the device functional layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a graph showing the light transmittance test results of sample paper prepared from cellulose with different beating degrees after being impregnated with epoxy resin according to Examples 1 to 3 of the preparation method of the composite film modified by epoxy resin of the present invention;

[0028] Figure 2 This is a graph showing the haze test results of sample paper prepared from cellulose with different beating degrees after being impregnated with epoxy resin according to Examples 1 to 3 of the method for preparing a composite film modified by epoxy resin of the present invention. DETAILED DESCRIPTION

[0029] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0030] The present invention discloses a method for preparing a composite membrane modified by epoxy resin, which comprises preparing a cellulose pulp with a high beating degree, and obtaining a sample paper after vacuum filtration, and then impregnating the sample paper in epoxy resin, and curing the sample paper in a thermostat at room temperature to obtain a cellulose / epoxy resin composite membrane. The method specifically comprises the following steps:

[0031] Step 1: Take 30g of dry hardwood (cellulose content 40% to 50%) as raw fiber to prepare cellulose pulp with a beating degree of 70°SR to 90°SR, and the cellulose film is set to 40.0g / m 2A wet cellulose film is obtained by vacuum filtration process, and then a dried cellulose film (120 mm×120 mm×3.8 mm) is obtained by vacuum drying (85°C~95°C, 4 min~6 min). The cellulose film is put into a sealed bag and stored for later use.

[0032] Step 2: Pour an appropriate amount of E51 epoxy resin into a disposable culture dish and heat it to 35°C, add 1,8-diamino-3,6-dioxooctane curing agent into the disposable culture dish, put it into a magnetic stirrer (90rpm~110rpm, 3min~5min), and then quickly transfer the disposable culture dish to a vacuum drying oven (50℃~70℃, 5min~7min) for degassing to obtain epoxy resin slurry. The mass ratio of E51 epoxy resin to 1,8-diamino-3,6-dioxooctane curing agent is 9:1.

[0033] Step 3, the cellulose film prepared in step 1 is treated by a dip coating process, the cellulose film is completely immersed in the epoxy resin, and then the immersed cellulose film is lifted by tweezers and vertically hung in a constant temperature box (curing temperature: 20°C ~ 30°C, curing time: 20h ~ 30h) for curing, and a cellulose / epoxy resin composite film is obtained after the curing is completed.

[0034] Example 1

[0035] The preparation method of the composite film modified by epoxy resin of the present invention specifically comprises the following steps:

[0036] Step 1: Take 30g of dry mass of poplar wood as raw material fiber to prepare cellulose pulp with a beating degree of 90°SR, and the cellulose film weight is set to 40.0g / m 2 The wet cellulose film is obtained by vacuum filtration process, and then the dried cellulose film is obtained by vacuum drying (85°C, 4min). The cellulose film is put into a sealed bag and stored for later use.

[0037] Step 2, pour E51 epoxy resin into a disposable culture dish and heat it to 35°C, add 1,8-diamino-3,6-dioxooctane curing agent into the disposable culture dish, put it into a magnetic bar for magnetic stirring (90rpm, 3min), and then quickly transfer the disposable culture dish to a vacuum drying oven (50°C, 5min) for degassing to obtain epoxy resin slurry; wherein the mass ratio of E51 epoxy resin to 1,8-diamino-3,6-dioxooctane curing agent is 9:1.

[0038] Step 3, treat the cellulose film prepared in step 1 by a dip coating process, completely immerse the cellulose film in epoxy resin, then lift the immersed cellulose film with tweezers and hang it vertically in a constant temperature box (curing temperature: 20°C, curing time: 20h) for curing, and obtain a cellulose / epoxy resin composite film after curing.

[0039] Example 2

[0040] The preparation method of the composite film modified by epoxy resin of the present invention specifically comprises the following steps:

[0041] Step 1: Take 30g of dry mass of poplar wood as raw material fiber to prepare cellulose pulp with a beating degree of 80°SR, and the cellulose film weight is set to 40.0g / m 2 The wet cellulose film is obtained by vacuum filtration process, and then the dried cellulose film is obtained by vacuum drying (90°C, 5min). The cellulose film is put into a sealed bag and stored for later use.

[0042] Step 2, pour E51 epoxy resin into a disposable culture dish and heat it to 35°C, add 1,8-diamino-3,6-dioxooctane curing agent into the disposable culture dish, put it into a magnetic bar for magnetic stirring (100 rpm, 4 minutes), and then quickly transfer the disposable culture dish to a vacuum drying oven (60°C, 6 minutes) for degassing to obtain epoxy resin slurry; wherein the mass ratio of E51 epoxy resin to 1,8-diamino-3,6-dioxooctane curing agent is 9:1.

[0043] Step 3, treat the cellulose film prepared in step 1 by a dip coating process, completely immerse the cellulose film in epoxy resin, then lift the immersed cellulose film with tweezers and hang it vertically in a constant temperature box (curing temperature: 25°C, curing time: 25h) for curing, and obtain a cellulose / epoxy resin composite film after curing.

[0044] Example 3

[0045] The preparation method of the composite film modified by epoxy resin of the present invention specifically comprises the following steps:

[0046] Step 1: Take 30g of dry mass of poplar wood as raw material fiber to prepare cellulose pulp with a beating degree of 70°SR, and the cellulose film weight is set to 40.0g / m 2 The wet cellulose film is obtained by vacuum filtration process, and then the dried cellulose film is obtained by vacuum drying (95°C, 6min). The cellulose film is put into a sealed bag and stored for later use.

[0047] Step 2, pour E51 epoxy resin into a disposable culture dish and heat it to 35°C, add 1,8-diamino-3,6-dioxooctane curing agent into the disposable culture dish, put it into a magnetic bar for magnetic stirring (110rpm, 5min), and then quickly transfer the disposable culture dish to a vacuum drying oven (70°C, 7min) for degassing to obtain epoxy resin slurry; wherein the mass ratio of E51 epoxy resin to 1,8-diamino-3,6-dioxooctane curing agent is 9:1.

[0048] Step 3: The cellulose film prepared in step 1 is treated by a dip coating process, and the cellulose film is completely immersed in the epoxy resin. The immersed cellulose film is then lifted up with tweezers and vertically hung in a constant temperature box (curing temperature: 30°C, curing time: 30h) for curing. After the curing is completed, a cellulose / epoxy resin composite film is obtained.

[0049] Figure 1 This is a graph showing the light transmittance test results of sample paper prepared from cellulose with different beating degrees after being impregnated with epoxy resin according to Examples 1 to 3 of the preparation method of the composite film modified by epoxy resin of the present invention;

[0050] Figure 2 This is a graph showing the haze test results of sample paper prepared from cellulose with different beating degrees after being impregnated with epoxy resin according to Examples 1 to 3 of the method for preparing a composite film modified by epoxy resin of the present invention.

[0051] When the wavelength is 500nm and the beating degree is 90°SR (Example 1), the transmittance is as high as 95.7% and the haze is 43.1%. The transmittance and haze effects of the prepared composite film can meet the comprehensive use requirements (the composite film prepared by the present invention is used for OLED and needs to meet the requirements of high transmittance and low haze). When the composite film prepared by the present invention is subsequently applied to OLED devices, the corresponding OLED device current density, current efficiency, power efficiency and brightness can be improved.

Claims

1. A method for preparing a composite film modified by epoxy resin, characterized in that: The specific steps include: Step 1, preparing a cellulose film; Step 2, preparing epoxy resin slurry; Step 3, completely immersing the cellulose film prepared in step 1 into the epoxy resin slurry prepared in step 2, and curing the cellulose film in a constant temperature box to form a film, thereby obtaining a cellulose / epoxy resin composite film.

2. The method for preparing a composite film based on epoxy resin modification according to claim 1, characterized in that: The specific process of step 1 is as follows: Step 1.1, taking 30 g of absolutely dry hardwood as raw material fiber, preparing cellulose pulp with a beating degree of 70°SR to 90°SR; Step 1.2: Set the weight of the cellulose film to 40.0 g / m 2 The cellulose slurry obtained in step 1.1 is subjected to a vacuum filtration process to prepare a wet cellulose film, which is then subjected to vacuum drying to obtain a dried cellulose film. The cellulose film is placed in a sealed bag and stored at room temperature for later use.

3. The method for preparing a composite film based on epoxy resin modification according to claim 2, characterized in that: In the step 1.1, the cellulose content in the hardwood is 40% to 50%.

4. The method for preparing a composite film based on epoxy resin modification according to claim 2, characterized in that: In the step 1.2, the vacuum drying temperature is 85° C. to 95° C., and the vacuum drying time is 4 min to 6 min.

5. The method for preparing a composite film based on epoxy resin modification according to claim 2, characterized in that: The specific process of step 2 is: Pour E51 epoxy resin into a disposable culture dish and heat it to 35°C, add 1,8-diamino-3,6-dioxaoctane curing agent into the disposable culture dish, put a magnetic bar into the disposable culture dish for magnetic stirring, and then transfer the disposable culture dish to a vacuum drying oven for degassing to obtain epoxy resin slurry.

6. The method for preparing the composite film based on epoxy resin modification according to claim 5, characterized in that: In the step 2, the rotation speed of the magnetic stirring is 90 rpm to 110 rpm, and the time of the magnetic stirring is 3 min to 5 min.

7. The method for preparing a composite film based on epoxy resin modification according to claim 5, characterized in that: In the step 2, the drying temperature in the vacuum drying oven is 50° C. to 70° C., and the vacuum drying time is 5 min to 7 min.

8. The method for preparing a composite film based on epoxy resin modification according to claim 5, characterized in that: In the step 2, the mass ratio of E51 epoxy resin to 1,8-diamino-3,6-dioxaoctane curing agent is 9:

1.

9. The method for preparing a composite film based on epoxy resin modification according to claim 5, characterized in that: The specific process of step 3 is: completely immersing the cellulose film prepared in step 1 in the epoxy resin prepared in step 2, then lifting the immersed cellulose film with tweezers and hanging it vertically in a constant temperature box for curing, and obtaining a cellulose / epoxy resin composite film after curing.

10. Composite membrane based on epoxy resin modification, characterized in that: The composite film is prepared by the method for preparing the composite film based on epoxy resin modification according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Cellulose nano-fibril / epoxy resin composite film preparation method

    CN103396654A

  • Preparation method of cellulose membrane with high light transmittance and high haze

    CN114753175A

  • Method for adjusting light transmittance of paper by using nano-crystalline cellulose fibers

    CN117265906A