Preparation method and application of metal surface radionuclide uranium decontaminating agent composition
By using metal surface radionuclide uranium detergent compositions, including specific proportions of industrial soft water and surfactants, efficient metal surface radionuclide uranium detergent products are prepared, which solves the problem of difficult removal of radionuclide pollution on metal surfaces. It achieves efficient removal rate and stability, reducing harm to the environment and human beings.
Patent Information
- Application Number
- CN202410999010.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art is difficult to effectively remove radioactive uranium pollution on metal surfaces, resulting in continuous harm to the biological and ecological environment.
Using a metal surface radionuclide uranium detergent composition, including industrial soft water, ethylenediaminetetraacetic acid, ethylenediaminetetraethyloxime, ethanol, alkyl polyglucoside, fatty alcohol polyoxygen with HLB value of 7 to 9 Vinyl ether, fatty alcohol polyoxyethylene ether and triethanolamine with HLB values of 10 to 15 are prepared by specific stirring and heating processes, and the metal surface radionuclide uranium detergent products are combined through fatty alcohol polyoxyethylene ether phosphate Modification improves decontamination efficiency.
The efficient removal of radionuclides on metal surfaces is achieved, with a removal rate of more than 97%, reducing the harm to the environment and humans, and improving the stability and compatibility of detergent products.
Smart Images

Figure CN118942755A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cleaning products, and more specifically, relates to a preparation method and application of a metal surface radioactive nuclide uranium cleaning agent composition. Background Art
[0002] Radioactive uranium is a key raw material for nuclear power generation. During nuclear power production, operation of nuclear facilities, post-processing procedures and use in related industries, it will contaminate the surfaces of various special metals. If the contamination of radioactive uranium on the metal surface cannot be removed in a timely and effective manner, it will inevitably seriously affect the safety of organisms (especially workers) and the ecological environment. Therefore, it has become a key issue that countries urgently need to solve.
[0003] Radioactive uranium has a long decay period, high chemical toxicity, and long-lasting toxicity, which not only pollutes the ecological environment, but also causes serious harm to the human body. Therefore, a special decontamination agent for radioactive uranium contamination on metal surfaces is developed to minimize the amount of radioactive uranium on metal surfaces during production, use, and post-processing, and avoid continuous damage to the environment and human body. Summary of the invention
[0004] An object of the present invention is to solve at least the above problems and / or disadvantages and to provide at least the advantages which will be described hereinafter.
[0005] In order to achieve these purposes and other advantages according to the present invention, a metal surface radioactive nuclide uranium decontamination composition is provided, comprising: industrial soft water, ethylenediaminetetraacetic acid, ethylenediaminetetraacetoxime, ethanol, alkyl polyglucoside, fatty alcohol polyoxyethylene ether with an HLB value of 7 to 9, fatty alcohol polyoxyethylene ether with an HLB value of 10 to 15, and triethanolamine.
[0006] Preferably, the mass proportion of ethylenediaminetetraacetic acid is 0.1-10%, the mass proportion of ethylenediaminetetraacetic acid is 0.1-10%, the mass proportion of ethanol is 1-10%, the mass proportion of alkyl polyglucoside is 0.1-20%, the mass proportion of fatty alcohol polyoxyethylene ether with an HLB value of 7-9 is 0.5-20%, the mass proportion of fatty alcohol polyoxyethylene ether with an HLB value of 10-15 is 1-20%, the mass proportion of triethanolamine is 0.1-5%, and the rest is industrial soft water.
[0007] Preferably, the mass proportion of ethylenediaminetetraacetic acid is 1-2%, the mass proportion of ethylenediaminetetraacetic acid is 5%, the mass proportion of ethanol is 8%, the mass proportion of alkyl polyglucoside is 2.15%, the mass proportion of fatty alcohol polyoxyethylene ether with an HLB value of 7-9 is 1%, the mass proportion of fatty alcohol polyoxyethylene ether with an HLB value of 10-15 is 2.15%, the mass proportion of triethanolamine is 1%, and the rest is industrial soft water.
[0008] Preferably, the structural formula of the ethylenediaminetetraethoxime is as follows:
[0009]
[0010] Add ethylenediamine and distilled water to a reaction container and stir at room temperature for 5 to 15 minutes, then adjust the temperature to 30 to 50°C, immediately add acrylonitrile and cover with a glass stopper, and obtain a light yellow clear solution after stirring for 1 hour; heat the light yellow clear solution to 60 to 80°C and continue stirring for 24 to 72 hours; after the stirring is completed, obtain a yellow clear solution, cool the yellow clear solution to room temperature, add ethanol and continue stirring, stir for 5 to 15 minutes, filter and obtain white needle-shaped N, N, N', N'-tetrakis (2-cyanoethyl) ethylenediamine, and finally dry in an oven at 30 to 50°C; wherein the volume ratio of ethylenediamine, distilled water, acrylonitrile and ethanol is 13 to 15:180 to 220:75 to 85:60 to 200;
[0011] N, N, N', N'-tetra(2-cyanoethyl)ethylenediamine is added to a solvent, wherein the volume ratio of water to acetonitrile in the solvent is 1:1, and hydroxylamine hydrochloride is added. When the hydroxylamine hydrochloride is fully dissolved, the pH value of the solution is measured using a pH meter, and then anhydrous sodium carbonate is added to the solution to adjust the pH value to 8, and then the solution is refluxed at 60-80° C. for 12-36 hours; finally, the refluxed product is added with ethanol of an equal volume to the solution, and then fully stirred to obtain a white precipitate, and finally centrifuged and dried to obtain ethylenediaminetetraethyloxime; wherein the mass volume ratio of N, N, N', N'-tetra(2-cyanoethyl)ethylenediamine, the solvent, and the hydroxylamine hydrochloride is 15-20 g:80-150 ml:16-20 g.
[0012] A metal surface radioactive nuclide uranium decontamination product contains a metal surface radioactive nuclide uranium decontamination composition.
[0013] Preferably, the metal surface radionuclide uranium decontamination product is a liquid detergent, and is prepared from a metal surface radionuclide uranium decontamination composition.
[0014] Preferably, the metal surface radioactive nuclide uranium decontamination product is used for decontamination of radioactive nuclide uranium on metal surfaces.
[0015] A method for preparing a metal surface radioactive nuclide uranium decontamination product, characterized in that it comprises the following steps:
[0016] S1. Place industrial soft water into a preparation container;
[0017] S2. Heat industrial soft water to 20-45°C, stir at a speed of 60-800 rpm, and add the remaining raw materials of the cleaning agent of the claim to the industrial soft water in the following order: ethanol, ethylenediaminetetraacetic acid, ethylenediaminetetraacetic oxime, alkyl polyglucoside, fatty alcohol polyoxyethylene ether with an HLB value of 10-15, and fatty alcohol polyoxyethylene ether with an HLB value of 7-9; the subsequent raw materials can be added in the above order only after the previous raw materials are fully dissolved and uniformly dissolved;
[0018] S3. During the preparation process, use an ordinary mixer or emulsifier to homogenize all the raw materials. The stirring time must be ≥ 3 minutes to obtain a metal surface radioactive nuclide uranium decontamination product.
[0019] Preferably, in said S1, the heating temperature of industrial soft water is 20-45° C., and the stirring speed is 60-800 rpm.
[0020] Preferably, in said S2, after the fatty alcohol polyoxyethylene ether with an HLB value of 7 to 9 is added, triethanolamine is finally added to adjust the metal surface radioactive nuclide uranium decontamination product to a neutral solution.
[0021] In order to improve the cleaning efficiency of radioactive uranium on metal surface by a metal surface radioactive nuclide uranium decontamination product, after preparing ethylenediaminetetraethyloxime, fatty alcohol polyoxyethylene ether phosphate and ethylenediaminetetraethyloxime are compounded and modified, and the specific method includes:
[0022] Dissolve ethylenediaminetetraethyloxime in deionized water, stir until dissolved, heat to 40-60°C, add fatty alcohol polyoxyethylene ether phosphate to the solution, stir at 200-600rpm, continue to heat to 60-90°C after the addition, keep warm for 20-60min, cool to room temperature, add ethanol of equal volume to the solution, stir to obtain white precipitate, centrifuge and dry to obtain ethylenediaminetetraethyloxime modified by fatty alcohol polyoxyethylene ether phosphate. The mass volume ratio of ethylenediaminetetraethyloxime, deionized water, and fatty alcohol polyoxyethylene ether phosphate is 10-20g:100-250mL:1-5g.
[0023] The present invention at least has the following beneficial effects: the metal surface radionuclide uranium decontamination product of the present invention can be conveniently and efficiently used for decontamination of radionuclide contamination on metal surfaces. The cleaning agent provided by the present invention includes the following raw materials in weight in addition to water: 0.1-10% of ethylenediaminetetraacetic acid, 0.1-10% of ethylenediaminetetraacetic acid, 1-10% of ethanol, 0.1-20% of alkyl polyglucoside, 1-20% of fatty alcohol polyoxyethylene ether (HLB value is 10-15), 0.5-20% of fatty alcohol polyoxyethylene ether (HLB value is 7-9) and 0.1-5% of triethanolamine. The metal surface radionuclide uranium decontamination product prepared by the present invention can remove more than 97% of the radionuclide within 3-5 minutes for cleaning the metal surface contaminated by radionuclide uranium. The metal surface radionuclide uranium decontamination product provided by the present invention can be used to specifically clean the pollution of radionuclide on the metal surface, and minimize the harm it brings to the environment and humans.
[0024] The present invention also uses fatty alcohol polyoxyethylene ether phosphate to compound and modify the prepared ethylenediaminetetraethyloxime, which not only improves the compatibility of ethylenediaminetetraethyloxime with fatty alcohol polyoxyethylene ethers with HLB values of 11-15 and fatty alcohol polyoxyethylene ethers with HLB values of 7-10, thereby improving the stability of the metal surface radionuclide uranium decontamination product, but also improves the surface activity of ethylenediaminetetraethyloxime and the metal surface radionuclide uranium decontamination product, and further improves the cleaning and removal ability of the metal surface radionuclide uranium decontamination product on the metal surface radionuclide.
[0025] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a microscopic morphology image of ethylenediaminetetraethyloxime used in Example 1 of the present invention magnified 500 times;
[0027] Figure 2 This is a microscopic morphology image of ethylenediaminetetraethyloxime used in Example 1 of the present invention magnified 2000 times;
[0028] Figure 3 is a TGA thermal analysis diagram of ethylenediaminetetraethyloxime used in Example 1 of the present invention;
[0029] Figure 4 The experimental data of the removal rate of nuclides from the metal sheet surface cleaning in Example 1 of the present invention. DETAILED DESCRIPTION
[0030] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.
[0031] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.
[0032] Example 1
[0033] This embodiment provides a metal surface radionuclide uranium decontamination composition, comprising:
[0034] 18g ethylenediaminetetraacetic acid, 18g ethylenediaminetetraacetic oxime, 18g ethanol, 36g alkyl polyglucoside, 36g fatty alcohol polyoxyethylene ether with HLB value of 10-15, 36g fatty alcohol polyoxyethylene ether with HLB value of 7-9 and 18g triethanolamine, and the rest is 820g industrial soft water.
[0035] The preparation method of ethylenediaminetetraethyloxime is:
[0036] Preparation of N, N, N', N'-tetrakis (2-cyanoethyl) ethylenediamine (CN-EDA):
[0037] First, build a three-necked flask and a condenser reflux device and flush it with nitrogen. After completion, seal it. The opening of the built condenser is sealed with a balloon, and the two sides of the three-necked flask are sealed with glass stoppers. Add 13.3ml (0.2mol) of ethylenediamine and 200ml of distilled water to the three-necked flask and stir at room temperature for 10min. Then adjust the temperature to 40℃ and immediately add 79ml (1.2mol) of acrylonitrile and cover it with a glass stopper. After about 1min, the solution begins to react violently. At this time, the air pressure in the container rises rapidly. After stirring for 1h, a light yellow clear solution can be obtained. Thereafter, the solution is heated to 70℃ and stirred for 48h. After stirring, a yellow clear solution is obtained. The solution is cooled to room temperature and poured into a large beaker. 100ml of ethanol is added and stirred continuously. A white precipitate will be produced after the yellow solution contacts the air. The white precipitate is easier to precipitate after adding ethanol. After stirring for 10min, it is filtered to obtain white needle-shaped N, N, N', N'-tetra (2-cyanoethyl) ethylenediamine, and finally dried in an oven at 40℃.
[0038] Preparation of ethylenediaminetetraethyloxime (AO-EDA):
[0039] Weigh 15.25g of N, N, N', N'-tetra(2-cyanoethyl)ethylenediamine, add 100ml of solvent (the volume ratio of water to acetonitrile is 1:1), and add 17.38g of hydroxylamine hydrochloride. When the hydroxylamine hydrochloride is fully dissolved, measure the pH value of the solution with a pH meter, then add anhydrous sodium carbonate to the solution to adjust the pH value to 8, and then reflux the solution at 70°C for 24h. Finally, add the above product to an equal volume of ethanol to the solution, then stir thoroughly to obtain a white precipitate, and finally centrifuge and dry to obtain a white powdery solid, which is ethylenediaminetetraethyloxime, and its structural formula is:
[0040]
[0041] The microscopic morphology images of ethylenediaminetetraethyloxime used in this embodiment at 500 times and 2000 times magnification are shown as follows: Figure 1 and Figure 2 As shown in the figure, it can be seen that:
[0042] The TGA thermal analysis diagram of ethylenediaminetetraethyloxime used in this example is as follows: Figure 3 shown.
[0043] The specific method of using the above-mentioned metal surface radionuclide uranium decontamination composition to prepare a metal surface radionuclide uranium decontamination product in this embodiment includes:
[0044] S1. Place industrial soft water into a preparation container;
[0045] S2. Heat industrial soft water to 30°C, stir at a speed of 400 rpm, and add the remaining raw materials of the cleaning agent of the claim to the industrial soft water in the following order: ethanol, ethylenediaminetetraacetic acid, ethylenediaminetetraethyloxime, alkyl polyglucoside, fatty alcohol polyoxyethylene ether with an HLB value of 10 to 15, and fatty alcohol polyoxyethylene ether with an HLB value of 7 to 9; the subsequent raw materials can be added in the above order only after the previous raw materials are fully dissolved;
[0046] S3. During the preparation process, all the raw materials are homogenized using a common mixer or emulsifier for 3 minutes to obtain a metal surface radioactive nuclide uranium decontamination product.
[0047] Preparation of metal sheets:
[0048] The length×width×height (thickness) of the metal sheet is high or medium carbon structural steel with a specification of 10cm×10cm×0.5cm.
[0049] 10 ml of the metal surface radioactive nuclide uranium decontamination product prepared in this example is added into 100 ml of water and mixed evenly.
[0050] Prepare a radioactive uranium solution of a certain concentration. Make sure to follow the safety protocols for all radioactive materials during the operation. Place the metal sheet on the laboratory workbench and detect the initial radioactivity value of the metal sheet. Use a dropper to evenly add 1L of 200mg / L radioactive uranium solution to a series of metal sheets, dry naturally in the shade, and place for 1d to 30d. Then put the metal sheets with different placement times into the container of metal surface radioactive nuclide uranium decontamination products, put them in an oscillator to shake and wash for 5 minutes, take out the metal sheet and rinse it with a spray bottle filled with clean water for 1 minute, and use the RJ39-2060 surface contamination meter to detect the radioactivity of its surface after drying, and monitor the background and the beta-ray counting rate before and after decontamination. The results show that the decontamination efficiency (decontamination rate) of this decontamination solution for radioactive nuclide uranium on the surface of the metal sheet is higher than 97%.
[0051] The calculation formula for the decontamination efficiency of radioactive nuclide uranium on the surface of the metal sheet is:
[0052] (β-ray counting rate before decontamination - β-ray counting rate after decontamination) / (β-ray counting rate before decontamination - background β-ray counting rate)×100%.
[0053] The experimental data of the removal rate of the core element after cleaning the metal sheet surface for 5 minutes is as follows Figure 4 shown.
[0054] Example 2
[0055] This embodiment provides a metal surface radionuclide uranium decontamination composition, comprising:
[0056] 15g ethylenediaminetetraacetic acid, 15g ethylenediaminetetraacetic oxime, 15g ethanol, 30g alkyl polyglucoside, 32g fatty alcohol polyoxyethylene ether with HLB value of 10-15, 35g fatty alcohol polyoxyethylene ether with HLB value of 7-9 and 8g triethanolamine, and the rest is 850g industrial soft water.
[0057] The method for preparing the metal surface radionuclide uranium decontamination product using the metal surface radionuclide uranium decontamination composition in this example is the same as that in Example 1.
[0058] Example 3
[0059] This embodiment provides a metal surface radionuclide uranium decontamination composition, comprising:
[0060] 10g ethylenediaminetetraacetic acid, 10g ethylenediaminetetraacetic oxime, 10g ethanol, 20g alkyl polyglucoside, 22g fatty alcohol polyoxyethylene ether with HLB value of 10-15, 25g fatty alcohol polyoxyethylene ether with HLB value of 7-9 and 3g triethanolamine, and the rest is 900g industrial soft water.
[0061] The method for preparing the metal surface radionuclide uranium decontamination product using the metal surface radionuclide uranium decontamination composition in this example is the same as that in Example 1.
[0062] Example 4
[0063] This embodiment provides a metal surface radioactive nuclide uranium decontamination composition, wherein the ethylenediaminetetraethyloxime in Example 1 is replaced by ethylenediaminetetraethyloxime modified by compounding with fatty alcohol polyoxyethylene ether phosphate of the same mass, and the remaining components and the preparation method of the metal surface radioactive nuclide uranium decontamination product are the same as those in Example 1; wherein the specific method of compounding and modifying ethylenediaminetetraethyloxime with fatty alcohol polyoxyethylene ether phosphate includes:
[0064] Dissolve 20 g of ethylenediaminetetraethyloxime in 250 mL of deionized water, stir until dissolved, heat to 50°C, add 5 g of fatty alcohol polyoxyethylene ether phosphate dropwise to the solution, and stir at 600 rpm while adding. After the addition is completed, continue to heat to 90°C, keep warm for 20 minutes, cool to room temperature, add ethanol in an amount equal to the volume of the solution, stir to obtain a white precipitate, and centrifuge and dry to obtain ethylenediaminetetraethyloxime composite-modified with fatty alcohol polyoxyethylene ether phosphate.
[0065] The same method as in Example 1 was used to detect the decontamination efficiency of the metal surface radioactive nuclide uranium decontamination product prepared in this example on the radioactive nuclide uranium contaminated metal sheet, and the specifications of the cleaned metal sheet were the same as in Example 1, namely:
[0066] Prepare a radioactive uranium solution of a certain concentration. Make sure to follow the safety protocols for all radioactive materials during the operation. Place the metal sheet on the laboratory workbench and detect the initial radioactivity value of the metal sheet. Use a dropper to evenly add 1L of 200mg / L radioactive uranium solution to a series of metal sheets, dry naturally in the shade, and place for 1d to 30d. Then put the metal sheets with different placement times into the container of radioactive nuclide uranium decontamination products on the metal surface, put them in an oscillator to vibrate and wash for 5 minutes, take out the metal sheet and rinse it with a spray bottle filled with clean water for 1 minute, and use the RJ39-2060 surface contamination meter to detect the radioactivity of its surface after drying, and monitor the background and the beta-ray count rate before and after decontamination. The results show that the decontamination efficiency of this decontamination solution for radioactive nuclide uranium on the surface of metal sheets is higher than 97.4%.
[0067] Among them, for the metal sheets placed for 10 days, 20 days and 30 days, the metal surface radionuclide uranium decontamination product prepared in this embodiment has a decontamination efficiency (decontamination rate) of 98.6%, 97.8% and 97.5% for radionuclide uranium, respectively, which are all higher than the corresponding decontamination efficiency of Example 1, indicating that the metal surface radionuclide uranium decontamination product prepared in this embodiment has a stronger radionuclide cleaning and removal ability for the metal sheet contaminated with radionuclides.
[0068] The number of devices and processing scales described here are used to simplify the description of the present invention. Applications, modifications and variations of the present invention will be obvious to those skilled in the art.
[0069] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes, and they can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.
Claims
1. A metal surface radionuclide uranium decontamination composition, characterized in that: include: Industrial soft water, ethylenediaminetetraacetic acid, ethylenediaminetetraacetic oxime, ethanol, alkyl polyglucoside, fatty alcohol polyoxyethylene ether with HLB value of 7-9, fatty alcohol polyoxyethylene ether with HLB value of 10-15 and triethanolamine.
2. The metal surface radionuclide uranium decontamination composition according to claim 1, characterized in that: The mass proportion of the ethylenediaminetetraacetic acid is 0.1-10%, the mass proportion of ethylenediaminetetraacetic acid is 0.1-10%, the mass proportion of ethanol is 1-10%, the mass proportion of alkyl polyglucoside is 0.1-20%, the mass proportion of fatty alcohol polyoxyethylene ether with an HLB value of 7-9 is 0.5-20%, the mass proportion of fatty alcohol polyoxyethylene ether with an HLB value of 10-15 is 1-20%, the mass proportion of triethanolamine is 0.1-5%, and the rest is industrial soft water.
3. The metal surface radionuclide uranium decontamination composition according to claim 1, characterized in that: The mass proportion of ethylenediaminetetraacetic acid is 1-2%, the mass proportion of ethylenediaminetetraacetic acid is 5%, the mass proportion of ethanol is 8%, the mass proportion of alkyl polyglucoside is 2.15%, the mass proportion of fatty alcohol polyoxyethylene ether with an HLB value of 7-9 is 1%, the mass proportion of fatty alcohol polyoxyethylene ether with an HLB value of 10-15 is 2.15%, the mass proportion of triethanolamine is 1%, and the rest is industrial soft water.
4. The metal surface radionuclide uranium decontamination composition according to claim 1, characterized in that: The structural formula of the ethylenediaminetetraethyloxime is as follows: The preparation method of ethylenediaminetetraacetoxime comprises the following steps: adding ethylenediamine and distilled water to a reaction vessel and stirring at room temperature for 5 to 15 minutes; then adjusting the temperature to 30 to 50° C., immediately adding acrylonitrile, and covering with a glass stopper; and stirring for 1 hour to obtain a light yellow clear solution; heating the light yellow clear solution to 60 to 80° C. and continuing to stir for 24 to 72 hours; and obtaining a yellow clear solution after stirring; cooling the yellow clear solution to room temperature, adding ethanol, and continuing to stir for 5 to 15 minutes, and filtering to obtain white needle-shaped N,N,N',N'-tetra(2-cyanoethyl)ethylenediamine; and finally drying in an oven at 30 to 50° C.; wherein the volume ratio of ethylenediamine, distilled water, acrylonitrile, and ethanol is 13 to 15:180 to 220:75 to 85:60 to 200. N,N,N',N'-tetrakis(2-cyanoethyl)ethylenediamine is added to a solvent in which the volume ratio of water to acetonitrile is 1:
1. Hydroxylamine hydrochloride is added. When the hydroxylamine hydrochloride is fully dissolved, the pH value of the solution is measured using a pH meter. Anhydrous sodium carbonate is then added to the solution to adjust the pH value to 8. The solution is then refluxed at 60-80°C for 12-36 hours. Finally, the refluxed product is added with ethanol of an equal volume to the solution, and then fully stirred to obtain a white precipitate. Finally, the precipitate is centrifuged and dried to obtain ethylenediaminetetraethyloxime. The mass volume ratio of N,N,N',N'-tetrakis(2-cyanoethyl)ethylenediamine, solvent, and hydroxylamine hydrochloride is 15-20g:80-150ml:16-20g.
5. A metal surface radioactive nuclide uranium decontamination product, characterized in that: The decontamination product contains the metal surface radioactive nuclide uranium decontamination composition according to claim 2 or 3.
6. The metal surface radionuclide uranium decontamination product according to claim 5, characterized in that: The metal surface radionuclide uranium decontamination product is a liquid detergent, and is prepared from the metal surface radionuclide uranium decontamination composition according to claim 1 or 2.
7. Use of the metal surface radioactive nuclide uranium decontamination product according to claim 6, characterized in that: The metal surface radioactive nuclide uranium decontamination product is used for decontamination of radioactive nuclide uranium on metal surfaces.
8. A method for preparing a metal surface radioactive nuclide uranium decontamination product according to claim 6, characterized in that: The following steps are involved: S1. Place industrial soft water into a preparation container; S2. Heat industrial soft water to 20-45°C and stir at 60-800 rpm. Add the remaining raw materials of the disinfectant according to the claim to the industrial soft water in the following order: ethanol, ethylenediaminetetraacetic acid, ethylenediaminetetraacetic oxime, alkyl polyglucoside, fatty alcohol polyoxyethylene ether with an HLB value of 10-15, and fatty alcohol polyoxyethylene ether with an HLB value of 7-9; only add the subsequent raw materials in the above order after the previous raw materials are fully dissolved. S3. During the preparation process, use a common mixer or emulsifier to homogenize all the raw materials. The stirring time must be ≥ 3 minutes to obtain the metal surface radioactive nuclide uranium decontamination product.
9. The method for preparing a metal surface radioactive nuclide uranium decontamination product according to claim 8, characterized in that: In the above-mentioned S1, the heating temperature of industrial soft water is 20-45° C., and the stirring speed is 60-800 rpm.
10. The method for preparing a metal surface radioactive nuclide uranium decontamination product according to claim 8, characterized in that: In the above S2, after the fatty alcohol polyoxyethylene ether with an HLB value of 7 to 9 is added, triethanolamine is finally added to adjust the metal surface radioactive nuclide uranium decontamination product to a neutral solution.