Preparation method of positive electrode slurry suitable for battery cell of electronic cigarette, positive plate for electronic cigarette, battery cell and lithium ion battery
By adjusting the preparation steps and stirring conditions of the positive electrode slurry, an excellent conductive network is formed, which solves the problem of rapid attenuation of electronic cigarette battery capacity, extends the cycle life of lithium-ion batteries and improves the cell performance.
Patent Information
- Application Number
- CN202410994543.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
The lithium-ion battery cell for electronic cigarettes rapidly attenuates the capacity under the conditions of large and large current pulse discharge, resulting in a short cycle life and cannot meet the increasing user needs.
By adjusting the addition order and stirring and dispersion speed of each material in the preparation step of the positive electrode slurry, we ensure that each material is mixed uniformly, forming an excellent conductive network, reducing the risk of conductive agent aggregation, and improving the performance of the positive electrode sheet and battery cell.
It extends the cycle life of lithium-ion batteries for electronic cigarettes, improves the cycle performance of the battery cell under large and small pulse discharge, and reduces the surface resistance and AC internal resistance.
Smart Images

Figure BDA0004959863760000061 
Figure BDA0004959863760000071 
Figure BDA0004959863760000131
Abstract
Description
Technical Field
[0001] The present invention relates to the field of battery technology, and in particular to a method for preparing a positive electrode slurry suitable for an electronic cigarette battery cell, a positive electrode sheet for the electronic cigarette, a battery cell and a lithium ion battery. Background Art
[0002] As a substitute or supplement to burning tobacco, electronic cigarettes have developed rapidly because they can keep pace with the times and meet the requirements of the times. With the rise and popularity of electronic cigarettes, users have higher and higher requirements for the service life of electronic cigarettes. At present, most electronic cigarettes on the market use lithium-ion batteries, and the cycle life of lithium-ion batteries is related to the service life of electronic cigarettes.
[0003] Different from the use scenarios of conventional lithium-ion batteries, the battery cells for electronic cigarettes need to discharge with a large current when inhaling to provide energy for the heating module to heat up quickly. When stopping inhaling, a small current discharge is required to keep the heating module at a certain temperature, and a large and small current alternating pulse discharge phenomenon is formed between continuous inhalation. The capacity of the existing lithium-ion batteries for electronic cigarettes on the market shows a step-by-step decrease and rapid decay under the conditions of large and small current pulse discharge cycles (1.3C charging / 5C discharge for 10 seconds, 0.5C discharge for 270 seconds, standby for 1 minute, and alternate discharge to 3V). The cycle life is less than 500 weeks, and only 300 weeks at high temperatures. The short cycle life of existing electronic cigarettes cannot meet the increasing usage needs of users. Therefore, it is urgent to improve the cycle life of electronic cigarette batteries to better meet the increasing usage needs of users. Summary of the invention
[0004] In order to solve the problem that the capacity of electronic cigarette batteries and lithium ion batteries decay rapidly under large and small current pulse discharge, resulting in a short cycle life and difficulty in meeting the user's usage needs, and to improve the cycle performance and cycle life of electronic cigarette batteries and lithium ion batteries, the present invention provides a method for preparing a positive electrode slurry suitable for electronic cigarette batteries, a positive electrode sheet for electronic cigarettes, a battery cell and a lithium ion battery.
[0005] According to a first aspect of the present invention, there is provided a method for preparing a positive electrode slurry suitable for an electronic cigarette battery core, comprising the following steps:
[0006] S1. After the binder and the first solvent are pre-mixed, the mixture is stirred and dispersed at a revolution speed w1 and a rotation speed v1 for t1 minutes to obtain a glue solution;
[0007] S2. After the gel solution and the first conductive agent are premixed, the mixture is stirred and dispersed at a revolution speed w2 and a rotation speed v2 for t2 minutes to obtain a first conductive paste;
[0008] S3. After premixing the first conductive paste and the second conductive agent, stirring and dispersing them at a revolution speed w3 and a rotation speed v3 for t3 minutes to obtain a second conductive paste;
[0009] S4. After the second conductive slurry is premixed with the positive electrode active material, it is stirred and dispersed at a revolution speed w4 and a rotation speed v4 for t4 minutes to obtain a mixture;
[0010] S5. The mixture and the second solvent are stirred and dispersed at a revolution speed w5 and a rotation speed v5 for t5 minutes to obtain a positive electrode slurry;
[0011] w1=w2=w3=w4=w5=5~50rpm;
[0012] v1=v2=100~3000rpm, v3=v4=v5=300~3000rpm;
[0013] t1=t4=50~500, t2=t3=t5=10~100.
[0014] The performance of lithium-ion batteries is closely related to the homogenization process. The stirring and dispersion speed and time during the homogenization process are related to the homogenization effect, and the homogenization effect will directly affect the performance of the positive electrode, battery cell and battery.
[0015] The inventors found that the capacity of lithium-ion batteries for electronic cigarettes decays rapidly under the conditions of large and small current pulse discharge cycles. This is mainly because the conventional positive electrode has limited ion conduction capacity under large and small current pulse discharge, and the pressure difference is large when the current jumps from large to small, and polarization continues to accumulate, resulting in the rapid decay of the capacity of existing lithium-ion batteries for electronic cigarettes, which in turn affects the cycle performance and cycle life of lithium-ion batteries for electronic cigarettes.
[0016] The present invention regulates the order of adding each material in the preparation step of the positive electrode slurry and controls the revolution speed of each material during stirring and dispersing after mixing to be between 5 and 50 rpm, so that the revolution speed during stirring and dispersing in each step is the same, which can ensure that each material has a suitable shear force during the mixing process, and the mixing effect of each material is better, so that each material in the final positive electrode slurry is more uniform and stable, and the rotation speed in steps S3, S4, and S5 is kept consistent, which is not only conducive to the formation of a conductive network between different conductive agents, but also has a better homogenization effect between the conductive agent and the positive electrode active material, and at the same time, the rotation speed is The speed and time are controlled within a specific range, which can improve the homogenization effect and stability of the positive electrode slurry, make the dispersion uniformity of each material in the positive electrode slurry better, reduce the risk of agglomeration of the conductive agent, and help the conductive agent form an excellent conductive network. The positive electrode slurry prepared by the preparation method of the positive electrode slurry provided by the present invention is applied to the preparation of positive electrode sheets and batteries for electronic cigarettes, and lithium-ion batteries, which can reduce the surface resistance of the positive electrode sheet, the AC internal resistance of the battery cell, and the large and small current voltage difference, thereby improving the cycle performance of the battery cell for electronic cigarettes under large and small pulse discharges, and ultimately extending the cycle life of the lithium-ion battery for electronic cigarettes.
[0017] If the stirring and dispersing speed during the preparation of the positive electrode slurry is too fast and the time is too long, it will easily lead to low viscosity and poor stability of the positive electrode slurry, and the material in the slurry will settle too quickly. At the same time, the conductive agent will be sheared and broken into a short chain structure, making it difficult to form a good conductive network, which will lead to an increase in the surface resistance of the positive electrode sheet and a decrease in the cycle performance of the battery cell. If the stirring and dispersing speed during the preparation of the positive electrode slurry is too slow and the time is too short, it will make it difficult to fully stir the positive electrode slurry, and the conductive agent will easily agglomerate, which will lead to a significant increase in the surface resistance of the positive electrode sheet and a significant decrease in the cycle performance of the battery cell.
[0018] Preferably, calculated by mass ratio, binder: first conductive agent: second conductive agent: positive electrode active material = 0.2-2: 0.2-2: 0.12-1.2: 94.8-99.48.
[0019] Preferably, in S2, the first conductive agent is conductive carbon black (SP).
[0020] Preferably, in S3, the second conductive agent is a mixture of multi-walled carbon nanotubes (MWCNT) and single-walled carbon nanotubes (SWCNT) in a mass ratio of 0.1-1:0.02-0.2.
[0021] Compared with the positive electrode slurry using one or two of SP, MWCNT, and SWCNT as conductive agents, this solution uses a combination of SP+MWCNT+SWCNT as conductive agents and adds them in steps for stirring and dispersion, which is beneficial to reducing the film resistance of the prepared positive electrode sheet, making the internal resistance of the final battery cell and the difference between large and small currents and voltages smaller, and improving the cycle performance of the battery cell.
[0022] Preferably, in S1, the first solvent comprises N-methylpyrrolidone (NMP).
[0023] Preferably, in S1 , the binder includes polyvinylidene fluoride (PVDF).
[0024] Preferably, in S5, the second solvent includes N-methylpyrrolidone (NMP).
[0025] Preferably, in S1, the solid content of the glue solution is 1-10%, and the viscosity is 1000-10000 mPa·s.
[0026] Preferably, in S5, the positive electrode slurry has a solid content of 60-80% and a viscosity of 2000-6000 mPa·s.
[0027] The solid content and viscosity of the positive electrode slurry are affected by the content of the binder, the stirring dispersion speed and time. Taking the above-mentioned factors into consideration, the solid content and viscosity of the final positive electrode slurry are controlled within the above-mentioned range, which is beneficial to improving the coating performance of the positive electrode slurry and enabling the positive electrode slurry to better match the coating process.
[0028] If the solid content of the positive electrode slurry is too high, the viscosity of the positive electrode slurry will increase, resulting in a decrease in the coating uniformity of the positive electrode slurry; if the solid content of the positive electrode slurry is too low, it will lead to difficulties in coating and baking the positive electrode slurry, the positive electrode active coating will easily crack, the binder and the conductive agent will easily float, and ultimately lead to poor uniformity of the positive electrode sheet and low peeling force between the positive electrode active coating and the positive electrode collector.
[0029] If the viscosity of the positive electrode slurry is too high, its leveling property will be poor during the coating process of the positive electrode slurry, which will cause large fluctuations in the surface density of the positive electrode active coating obtained after coating the positive electrode slurry, making the uniformity of the prepared positive electrode sheet poor; if the viscosity of the positive electrode slurry is too low, severe tailing will occur during the coating process of the positive electrode slurry, thereby reducing the performance of the positive electrode sheet, battery cell and battery.
[0030] Preferably, in S4, the positive electrode active material is selected from at least one of lithium cobalt oxide materials and ternary positive electrode materials.
[0031] Preferably, the particle size D50 of the positive electrode active material is 5 to 10 μm, and the specific surface area is 0.1 to 0.5 m 2 / g, tap density is 2-3g / cm 3 .
[0032] Preferably, in S1, S2, S3 and S4, the premixing operation conditions are as follows: revolution speed 5 to 50 rpm, rotation speed 50 to 500 rpm, stirring and dispersing time 5 to 50 minutes.
[0033] Preferably, the premixing operation is carried out in a mixing tank, and after the premixing is completed, the materials on the wall of the mixing tank and the stirring paddle are scraped into the mixing system.
[0034] In the process of preparing the positive electrode slurry, pre-stirring and scraping the cylinder are first performed to avoid the area between the stirring slurry and the cylinder wall from being unable to be uniformly stirred and dispersed, which is beneficial to improving the particle size and fineness of the positive electrode slurry.
[0035] Preferably, during the stirring and dispersing operations of S1, S2, S3, S4 and S5, the reaction system is evacuated and the temperature of the reaction system is controlled to be 15-45°C.
[0036] Preferably, during the stirring and dispersing operations of S1, S2, S3, S4 and S5, the temperature of the reaction system is controlled by circulating cooling water.
[0037] During the preparation of the positive electrode slurry, vacuum treatment and cooling water operation are performed. Vacuuming can eliminate bubbles generated during the stirring and dispersing process of the positive electrode slurry, improve the quality of the positive electrode active coating formed after the positive electrode slurry is coated, and cooling water can ensure that the stirring temperature is within the range of 15 to 45°C, which can improve the stability of the positive electrode slurry.
[0038] The stirring and dispersing process is a process of continuous heat generation. If the temperature of the positive electrode slurry is not controlled during the stirring and dispersing process, the temperature of the system will become higher and higher as the stirring and dispersing process proceeds, and the viscosity of the positive electrode slurry will decrease. After the stirring and dispersing process is stopped, the viscosity of the positive electrode slurry will rebound severely, affecting the coating quality of the positive electrode slurry. If the temperature of the positive electrode slurry during the stirring and dispersing process is too low, the viscosity of the positive electrode slurry will be too high and the shearing effect will be too strong, which will be more destructive to the conductive agent, especially MWCNT and SWCNT, which is not conducive to homogenization and makes MWCNT and SWCNT easily sheared into short chain structures, affecting the formation of the conductive network, thereby deteriorating the performance of the positive electrode sheet and the battery cell.
[0039] According to a second aspect of the present invention, a positive electrode sheet for an electronic cigarette is provided, the positive electrode sheet comprising a positive electrode current collector and a positive electrode active coating, the positive electrode active coating is prepared from a positive electrode slurry, and the positive electrode slurry is prepared by the above-mentioned method for preparing a positive electrode slurry suitable for an electronic cigarette battery cell.
[0040] Preferably, the thickness of the positive electrode current collector is 8 to 16 μm.
[0041] Preferably, the surface density of the positive electrode active coating is 100 to 350 g / m 2 .
[0042] Preferably, the thickness of the positive electrode sheet is 33-103 μm.
[0043] According to a third aspect of the present invention, a battery cell for electronic cigarette is provided, and the battery cell comprises the above-mentioned positive electrode sheet for electronic cigarette.
[0044] According to a fourth aspect of the present invention, a lithium-ion battery for electronic cigarette is provided, and the lithium-ion battery includes the above-mentioned battery cell for electronic cigarette.
[0045] The positive electrode slurry prepared by the preparation method of the positive electrode slurry provided by the present invention is applied to the preparation of positive electrode sheets, battery cells and lithium ion batteries for electronic cigarettes, which can reduce the surface resistance of the positive electrode sheets, the AC internal resistance of the battery cells and the large and small current voltage difference, thereby improving the cycle performance of the battery cells for electronic cigarettes under large and small pulse discharges, and extending the cycle life of the lithium ion batteries for electronic cigarettes. DETAILED DESCRIPTION
[0046] The following is a further clear and complete description of the technical features in the technical solution provided by the present invention in conjunction with the specific implementation methods. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.
[0047] Examples 1 to 3
[0048] A lithium ion battery for electronic cigarettes, the preparation method of which comprises the following steps:
[0049] 1. Preparation of positive electrode
[0050] S1. Adding a binder polyvinylidene fluoride (PVDF) and a first solvent N-methylpyrrolidone (NMP) into a stirring tank, and after premixing, opening the stirring tank to scrape the binder on the tank wall and the stirring paddle into the first solvent, and then stirring and dispersing for t1 minute at a revolution speed w1 and a rotation speed v1 to obtain a glue solution with a solid content of 1 to 10% and a viscosity of 1000 to 10000 mPa·s;
[0051] S2. Add the first conductive agent to the above-mentioned glue solution, and after premixing, open the stirring cylinder to scrape the SP on the cylinder wall and the stirring paddle into the glue solution, and then stir and disperse for t2 minutes at the revolution speed w2 and the rotation speed v2 to obtain the first conductive slurry;
[0052] The first conductive agent is conductive carbon black (SP);
[0053] S3. The second conductive agent is added to the first conductive paste, pre-mixed, and then stirred and dispersed at a revolution speed w3 and a rotation speed v3 for t3 minutes to obtain a second conductive paste;
[0054] The second conductive agent is a mixture of multi-walled carbon nanotubes (MWCNT) and single-walled carbon nanotubes (SWCNT) in a mass ratio of 0.1-1:0.02-0.2;
[0055] S4. The positive electrode active material is added to the second conductive slurry, pre-mixed, and then stirred and dispersed at a revolution speed w4 and a rotation speed v4 for t4 minutes to obtain a mixture;
[0056] The positive electrode active material adopts a particle size D50 of 5 to 10 μm and a specific surface area of 0.1 to 0.5 m 2 / g, tap density is 2 to 3 g / cm 3 of lithium cobalt oxide;
[0057] S5. Add the second solvent NMP to the mixture and stir and disperse at revolution speed w5 and rotation speed v5 for t5 minutes to obtain a positive electrode slurry having a solid content of 60 to 80% and a viscosity of 2000 to 6000 mPa·s;
[0058] S6. The positive electrode slurry is coated on both surfaces of the positive electrode current collector aluminum foil (thickness of 10 μm) to form a surface density of 280 g / m 2 The positive electrode active coating is cold pressed and vacuum dried to obtain a positive electrode sheet with a thickness of 80 μm.
[0059] In S1, S2, S3, and S4, the conditions for the premixing operation are as follows: revolution speed 5 to 50 rpm, rotation speed 50 to 500 rpm, stirring and dispersing time 5 to 50 minutes;
[0060] Calculated by mass ratio, binder: first conductive agent: second conductive agent: positive electrode active material = 0.2-2: 0.2-2: 0.12-1.2: 94.8-99.48;
[0061] During the stirring and dispersing operation of S1, S2, S3, S4 and S5, the reaction system is evacuated and the cooling water circulation is turned on to control the temperature of the reaction system to be 15-45°C.
[0062] In Example 1, according to the mass ratio, the binder: the first conductive agent: the second conductive agent: the positive electrode active material = 2:2:1.2:94.8; the temperature of the reaction system was controlled to be 15°C.
[0063] In Example 2, according to the mass ratio, the binder: the first conductive agent: the second conductive agent: the positive electrode active material = 1:1:0.5:97.5; the temperature of the reaction system is controlled to be 30°C.
[0064] In Example 3, according to the mass ratio, the binder: the first conductive agent: the second conductive agent: the positive electrode active material = 0.2: 0.2: 0.12: 99.48; the temperature of the reaction system was controlled to be 45°C.
[0065] Table 1 Stirring and dispersion speed and time in the preparation method of positive electrode slurry of Examples 1 to 3
[0066]
[0067]
[0068] 2. Preparation of negative electrode
[0069] The negative electrode active material graphite, the binder sodium carboxymethyl cellulose (CMC), the styrene-butadiene rubber (SBR) and the conductive agent conductive carbon black (SP) were mixed in a mass ratio of 96:1.5:1.5:1 and added into the solvent deionized water, mixed evenly, to prepare a negative electrode slurry with a solid content of 48% and a viscosity of 2500 mPa·s. The negative electrode slurry was coated on both surfaces of the negative electrode current collector copper foil (thickness of 6 μm) to form a negative electrode active coating. After vacuum drying, a negative electrode sheet was prepared.
[0070] 3. Preparation of Diaphragm
[0071] A polyethylene film with a thickness of 8 μm was selected as the separator.
[0072] 4. Preparation of Electrolyte
[0073] Ethylene carbonate (EC), dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC) are mixed in a volume ratio of 1:1:1 to obtain an organic solvent, and then fully dried lithium salt LiPF6 is dissolved in the organic solvent to prepare an electrolyte with a concentration of 1M.
[0074] 5. Assembly of lithium-ion batteries
[0075] The positive electrode sheet, separator and negative electrode sheet are stacked in order, so that the separator is placed between the positive and negative electrode sheets to play an isolating role, and then wound to obtain a battery cell, which is placed in an outer packaging shell, and after drying, the above electrolyte is injected, and a lithium-ion battery is obtained through vacuum packaging, standing, forming, shaping and other processes.
[0076] Example 4
[0077] This embodiment provides a lithium-ion battery for electronic cigarettes. Compared with the embodiment 1, the difference in structure is that the type of conductive agent used in the preparation step S3 of the positive electrode sheet is different. Specifically, the second conductive agent used in this embodiment is SP. In addition to the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in the embodiment 1.
[0078] Example 5
[0079] This embodiment provides a lithium-ion battery for electronic cigarettes. Compared with the embodiment 1, the difference in structure is that the type of conductive agent used in the preparation step S3 of the positive electrode sheet is different. Specifically, the second conductive agent used in this embodiment is MWCNT. Except for the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in the embodiment 1.
[0080] Example 6
[0081] This embodiment provides a lithium-ion battery for electronic cigarettes. Compared with the embodiment 1, the difference in structure is that the type of conductive agent used in the preparation step S3 of the positive electrode sheet is different. Specifically, the second conductive agent used in this embodiment is SWCNT. Except for the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in the embodiment 1.
[0082] Example 7
[0083] This embodiment provides a lithium-ion battery for electronic cigarettes. Compared with the embodiment 1, the difference in structure is that the types of conductive agents used in the preparation steps S2 and S3 of the positive electrode sheet are different. Specifically, the first conductive agent used in this embodiment is MWCNT, and the second conductive agent is SWCNT. Except for the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in the embodiment 1.
[0084] Example 8
[0085] This embodiment provides a lithium-ion battery for electronic cigarettes. Compared with the embodiment 1, the difference in structure is that the types of conductive agents used in the preparation steps S2 and S3 of the positive electrode sheet are different. Specifically, the first conductive agent used in this embodiment is MWCNT+SWCNT, and the second conductive agent is SP. Except for the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in the embodiment 1.
[0086] Example 9
[0087] This embodiment provides a lithium-ion battery for electronic cigarettes. Compared with the embodiment 1, the difference in structure is that during the preparation of the positive electrode slurry, the reaction system is not vacuumed. In addition to the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in the embodiment 1.
[0088] Example 10
[0089] This embodiment provides a lithium-ion battery for electronic cigarettes. Compared with the embodiment 1, the difference in structure is that during the preparation of the positive electrode slurry, the cooling water circulation is not turned on, and the temperature of the reaction system exceeds 45° C. during the stirring and dispersion process. In addition to the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in the embodiment 1.
[0090] Embodiment 11
[0091] This embodiment provides a lithium ion battery for electronic cigarettes. Compared with the embodiment 1, the difference in structure is that during the preparation of the positive electrode slurry, the temperature of the reaction system is controlled to be lower than 15° C. In addition to the above differences, the materials, formula ratios and preparation operations used in this embodiment are strictly consistent with those in the embodiment 1.
[0092] Comparative Example 1
[0093] This comparative example provides a lithium-ion battery for an electronic cigarette. Compared with Example 1, the difference in structure is that in the process of preparing the positive electrode sheet, the preparation method of the positive electrode slurry is different.
[0094] The preparation method of the positive electrode sheet used in this comparative example is as follows:
[0095] S1. The polyvinylidene fluoride is uniformly added to the N-methylpyrrolidone solution, and the polyvinylidene fluoride glue solution is obtained by vacuum stirring, wherein the volume ratio of the polyvinylidene fluoride to the N-methylpyrrolidone solution is 1:14;
[0096] S2. adding a conductive agent to the polyvinylidene fluoride adhesive solution and dispersing the conductive agent uniformly to obtain a uniformly dispersed conductive adhesive solution, wherein the conductive agent is a mixture of conductive carbon black and single-walled carbon nanotubes in a mass ratio of 1:1;
[0097] S3. The positive electrode active material was evenly added to the conductive gel in portions, during which a solvent was added, and the mixture was stirred and dispersed at a revolution speed of 25 rpm and a rotation speed of 135 rpm for 30 min to obtain a primary kneaded slurry having a solid content of 75%;
[0098] S4. A solvent was added to the primary kneaded slurry, and the mixture was stirred and dispersed at a revolution speed of 25 rpm and a rotation speed of 160 rpm for 30 min to obtain a secondary kneaded slurry having a solid content of 73%;
[0099] S5. The secondary kneaded slurry was stirred and dispersed at a revolution speed of 35 rpm and a rotation speed of 3500 rpm to obtain a positive electrode slurry having a viscosity of 6500 mPa·s and a solid content of 67%;
[0100] S6. The positive electrode slurry is coated on both surfaces of the positive electrode current collector aluminum foil (thickness of 10 μm) to form a surface density of 280 g / m 2 The positive electrode active coating is cold pressed and vacuum dried to obtain a positive electrode sheet with a thickness of 80μm.
[0101] Except for the above differences, the materials, formula ratios and preparation operations used in this comparative example are strictly consistent with those in Example 1.
[0102] Comparative Example 2
[0103] This comparative example provides a lithium-ion battery for electronic cigarettes. Compared with Example 1, the difference in structure is that in the preparation steps S1, S2, S3, and S4 of the positive electrode sheet, the premixing step is omitted. Except for the above difference, the materials, formula ratios, and preparation operations used in this comparative example are strictly consistent with those in Example 1.
[0104] Comparative Example 3
[0105] This comparative example provides a lithium-ion battery for electronic cigarettes. Compared with Example 1, the difference in structure is that the stirring and dispersion speed in the preparation process of the positive electrode sheet is different. Specifically, in this comparative example, w1=w2=w3=w4=w5=3rpm; v1=v2=80rpm, v3=v4=v5=250rpm. Except for the above differences, the materials, formula ratios and preparation operations used in this comparative example are strictly consistent with those in Example 1.
[0106] Comparative Example 4
[0107] This comparative example provides a lithium-ion battery for electronic cigarettes. Compared with Example 1, the difference in structure is that the stirring and dispersion speed in the preparation process of the positive electrode sheet is different. Specifically, in this comparative example, w1=w2=w3=w4=w5=60rpm; v1=v2=3100rpm, v3=v4=v5=3100rpm. Except for the above differences, the materials, formula ratios and preparation operations used in this comparative example are strictly consistent with those in Example 1.
[0108] Comparative Example 5
[0109] This comparative example provides a lithium-ion battery for electronic cigarettes. Compared with Example 1, the difference in structure is that the stirring and dispersion time in the preparation process of the positive electrode sheet is different. Specifically, in this comparative example, t1=t4=40min, t2=t3=t5=5min. Except for the above differences, the materials, formula ratios and preparation operations used in this comparative example are strictly consistent with those in Example 1.
[0110] Comparative Example 6
[0111] This comparative example provides a lithium-ion battery for electronic cigarettes. Compared with Example 1, the difference in structure is that the stirring and dispersion time in the preparation process of the positive electrode sheet is different. Specifically, in this comparative example, t1=t4=510min, t2=t3=t5=110min. Except for the above differences, the materials, formula ratios and preparation operations used in this comparative example are strictly consistent with those in Example 1.
[0112] Test Case
[0113] 1. Participants
[0114] In this test example, the positive electrode sheets, cells and batteries prepared in Examples 1 to 11 and Comparative Examples 1 to 6 were used as test objects to conduct relevant performance tests.
[0115] 2. Test content
[0116] (1) Surface resistivity of the positive electrode
[0117] At a temperature of 25±2°C, the electrode sheet resistance test system was used with a pressure set to 20MPa and a pressure holding time of 20s to test the surface resistance of the positive electrode sheet after drying the positive electrode active coating and before cold pressing, and the surface resistivity of the positive electrode sheet was calculated.
[0118] (2) Internal resistance of battery cell
[0119] At a temperature of 25±2° C., the lithium-ion battery was charged at a constant current of 0.5C to a state of charge SOC=50%, and the internal resistance of the battery cell was obtained by using a voltage internal resistance meter.
[0120] (3) Current and voltage difference
[0121] At a temperature of 25±2°C, the lithium-ion battery is charged to a full charge state (cut-off current 0.05C) at a constant current and constant voltage rate of 1.3C, and then left for 5 minutes. The lithium-ion battery is discharged at a constant current rate of 5C for 10 seconds, and then the lithium-ion battery is discharged at a constant current rate of 0.5C for 270 seconds, and left for 1 minute. The lithium-ion battery is discharged at a constant current rate of 5C for 10 seconds, and the lithium-ion battery is discharged at a constant current rate of 0.5C for 270 seconds, and left for 1 minute. The discharge is repeated to 3V, and the voltage at the 10th second of 5C discharge and the voltage at the beginning of 0.5C discharge before stopping the discharge are recorded. The difference between the two is taken as the voltage difference of the battery under large (5C) and small (0.5C) currents.
[0122] (4) 5C / 10C rate discharge capacity retention
[0123] At a temperature of 25±2℃, the lithium-ion battery was charged with constant current and constant voltage at a rate of 0.5C to a full charge state (cut-off current 0.05C), left for 5 minutes, and discharged to 3V at currents of 1C / 5C / 10C, respectively. The 1C / 5C / 10C discharge capacities were recorded, and the ratio of the 5C / 10C discharge capacity to the 1C discharge capacity was taken as the 5C / 10C rate discharge capacity retention rate.
[0124] (5) Capacity retention rate of pulse discharge cycles with large and small currents at different temperatures
[0125] The batteries prepared in Examples 1 to 11 and Comparative Examples 1 to 6 were charged at different temperatures (25°C, 45°C, 50°C, and 55°C) at a constant current and constant voltage rate of 1.3C to a full charge state (cut-off current 0.05C), left for 5 minutes, and then discharged at a constant current rate of 5C for 10 seconds, and then discharged at a constant current rate of 0.5C for 270 seconds, left for 1 minute, and then discharged at a constant current rate of 5C for 10 seconds. , the lithium-ion battery is discharged at a constant current of 0.5C rate for 270 seconds, left for 1 minute, and repeatedly discharged to 3V, which is regarded as one charge and discharge cycle, and the discharge capacity of the lithium-ion battery is tested before and after 800 cycles of charge and discharge. The capacity retention rate of the lithium-ion battery after 800 cycles of charge and discharge is calculated according to the following formula: 800-week capacity retention rate = (discharge capacity of the 800th cycle / first discharge capacity) × 100%; or the number of cycles when the capacity retention rate of the lithium-ion battery is less than 80%.
[0126] In the capacity retention test results of lithium-ion batteries, the capacity retention rate and the number of cycles are correlated, and the specific expression method of the test results is as follows: for example, if the capacity retention rate is 87.8% after 800 cycles at 25°C, it is recorded as 87.8%@800 weeks; if the capacity retention rate is 80% after 700 cycles at 55°C, it is recorded as 80%@700 weeks.
[0127] 3. Experimental results
[0128] Table 1 Surface resistivity test results of positive electrode sheet before cold pressing
[0129] Group <![CDATA[Sheet resistivity (mΩ / mm 2 )]]> Example 1 2.23 Example 2 2.21 Example 3 2.36 Example 4 7.03 Example 5 4.17 Example 6 4.14 Example 7 6.15 Example 8 5.22 Example 9 3.56 Example 10 3.35 Embodiment 11 7.38 Comparative Example 1 7.96 Comparative Example 2 7.70 Comparative Example 3 9.16 Comparative Example 4 7.86 Comparative Example 5 7.82 Comparative Example 6 7.89
[0130] Table 2 Test results of relevant performance of cells and batteries
[0131]
[0132] The surface resistivity test results of the positive electrode sheets prepared in Examples 1 to 11 and Comparative Examples 1 to 6 before cold pressing are shown in Table 1, and the relevant performance test results of the cells and batteries prepared in Examples 1 to 11 and Comparative Examples 1 to 6 are shown in Table 2.
[0133] Compared with Comparative Examples 1 to 6, the surface resistivity of the positive electrode sheets prepared in Examples 1 to 11 before cold pressing, the internal resistance of the battery cells, and the large and small current voltage difference of the lithium ion batteries are all lower than those of Comparative Examples 1 to 6, and the discharge capacity retention rate of the lithium ion batteries prepared in Examples 1 to 11 at 5C and 10C rates and the cycle capacity retention rate of large and small current pulse discharge at 25 to 55°C are all higher than those of Comparative Examples 1 to 6. The main reason for the above phenomenon is that the positive electrode slurry used in the preparation process of the positive electrode sheet of the lithium ion battery provided in Examples 1 to 11 is prepared by premixing a binder with a first solvent and then stirring and dispersing to obtain a glue solution, premixing the glue solution with a first conductive agent and then stirring and dispersing to obtain a first conductive slurry, then premixing the first conductive slurry with a second conductive agent and then stirring and dispersing to obtain a second conductive slurry, then premixing the second conductive slurry with a positive electrode active material and then stirring and dispersing to obtain a mixture, and finally mixing the mixture with a second solvent and stirring and dispersing it uniformly, and the positive electrode slurry is prepared by regulating the order of adding each material in the preparation step of the positive electrode slurry and mixing each material after stirring and dispersing. The revolution speed is controlled between 5 and 50 rpm, and the rotation speed and time are controlled within a specific range, which can improve the homogenization effect and stability of the positive electrode slurry, make the dispersion uniformity of each material in the positive electrode slurry better, reduce the risk of agglomeration of the conductive agent, and help the conductive agent form an excellent conductive network. The positive electrode slurry prepared by the preparation method of the positive electrode slurry provided by the present invention is applied to the preparation of positive electrode sheets and batteries for electronic cigarettes, and lithium-ion batteries, which can reduce the surface resistance of the positive electrode sheet, the AC internal resistance of the battery cell, and the large and small current voltage difference, thereby improving the cycle performance of the electronic cigarette battery cell under large and small pulse discharges, and ultimately extending the cycle life of the lithium-ion battery for electronic cigarettes.
[0134] Compared with Example 1, the positive electrode slurry used in the preparation process of the positive electrode sheet of the lithium ion battery provided in Examples 4 to 8 uses different types of the first conductive agent and / or the second conductive agent in the preparation process. The test results show that the surface resistivity of the positive electrode sheet prepared in Examples 4 to 8 before cold pressing, the internal resistance of the battery cell and the large and small current voltage difference of the lithium ion battery are all higher than those in Example 1, and the discharge capacity retention rate of the lithium ion battery prepared in Examples 4 to 8 at 5C and 10C rates and the cycle capacity retention rate of large and small current pulse discharge at 25 to 55°C are lower than those in Example 1. The above results show that the types of the first conductive agent and the second conductive agent will affect the performance of the positive electrode slurry and thus affect the performance of the positive electrode sheet, battery cell and lithium-ion battery obtained therefrom. Compared with the positive electrode slurry using one or two of SP, MWCNT and SWCNT as conductive agents, Example 1 uses SP as the first conductive agent, MWCNT and SWCNT as the second conductive agent and adds them step by step for stirring and dispersion, which is beneficial to reducing the membrane resistance of the obtained positive electrode sheet, making the internal resistance of the final battery cell and the difference between large and small currents and voltages smaller, and improving the cycle performance of the battery cell.
[0135] Compared with Example 1, in Example 9, the system was not vacuumed during the preparation of the positive electrode slurry. In Example 10, the cooling water circulation was not turned on during the preparation of the positive electrode slurry. The temperature of the reaction system exceeded 45°C during the stirring and dispersion of the slurry. In Example 11, the temperature of the reaction system was controlled to be lower than 15°C during the preparation of the positive electrode slurry. The test results showed that the surface resistivity, cell internal resistance and large current and voltage difference of the positive electrode sheets prepared in Examples 9 to 11 before cold pressing were higher than those in Example 1, and the discharge capacity retention rate of the lithium ion batteries prepared in Examples 9 to 11 at 5C and 10C rates and the cycle capacity retention rate of large and small current pulse discharge at 25 to 55°C were lower than those in Example 1. The main reasons for the above results are: vacuum treatment and cooling water operation are performed during the preparation of the positive electrode slurry. Vacuuming can eliminate bubbles generated during the stirring and dispersing process of the positive electrode slurry, and improve the quality of the positive electrode active coating formed after the positive electrode slurry is coated. Cooling water can ensure that the stirring temperature is in the range of 15 to 45°C, which can improve the stability of the positive electrode slurry. If the temperature during the stirring and dispersing process of the positive electrode slurry is not controlled, as the stirring and dispersing process proceeds, the temperature of the system will become higher and higher, and the viscosity of the positive electrode slurry will decrease. After the stirring and dispersing is stopped, the viscosity of the positive electrode slurry rebounds severely, affecting the coating quality of the positive electrode slurry. If the temperature during the stirring and dispersing process of the positive electrode slurry is too low, the viscosity of the positive electrode slurry will be too high, the shearing effect will be too strong, and the conductive agent, especially MWCNT and SWCNT, will be more destructive, which is not conducive to homogenization, and makes MWCNT and SWCNT easily sheared into short chain structures, which affects the formation of the conductive network, thereby deteriorating the performance of the positive electrode sheet and the battery cell.
[0136] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the protection scope of the present invention. Although the present invention is described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the technical solutions of the present invention can be modified or equivalently replaced, but these modifications or replacements are all within the protection scope of the present invention.
Claims
1. A method for preparing a positive electrode slurry suitable for an electronic cigarette battery core, characterized in that: The following steps are involved: S1. After the binder and the first solvent are pre-mixed, the mixture is stirred and dispersed at a revolution speed w1 and a rotation speed v1 for t1 minutes to obtain a glue solution; S2. After the glue solution is premixed with the first conductive agent, the mixture is stirred and dispersed at a revolution speed w2 and a rotation speed v2 for t2 minutes to obtain a first conductive paste; S3. After premixing the first conductive paste and the second conductive agent, stirring and dispersing them at a revolution speed w3 and a rotation speed v3 for t3 minutes to obtain a second conductive paste; S4. After premixing the second conductive slurry with the positive electrode active material, stirring and dispersing at a revolution speed w4 and a rotation speed v4 for t4 minutes to obtain a mixture; S5. The mixture and the second solvent are stirred and dispersed at a revolution speed w5 and a rotation speed v5 for t5 minutes to obtain the positive electrode slurry; w1=w2=w3=w4=w5=5~50rpm; v1=v2=100~3000rpm, v3=v4=v5=300~3000rpm; t1=t4=50~500, t2=t3=t5=10~100.
2. The method for preparing the positive electrode slurry suitable for the battery core for electronic cigarettes according to claim 1, characterized in that: Calculated by mass ratio, the binder: the first conductive agent: the second conductive agent: the positive electrode active material = 0.2-2: 0.2-2: 0.12-1.2: 94.8-99.
48.
3. The method for preparing the positive electrode slurry suitable for the battery core for electronic cigarettes according to claim 2, characterized in that: In S2, the first conductive agent is conductive carbon black, and / or, In S3, the second conductive agent is formed by mixing multi-walled carbon nanotubes and single-walled carbon nanotubes in a mass ratio of 0.1-1:0.02-0.
2.
4. The method for preparing the positive electrode slurry suitable for the battery core for electronic cigarettes according to claim 1, characterized in that: In S1, the first solvent includes N-methylpyrrolidone, the binder includes polyvinylidene fluoride, and / or, In the S5, the second solvent includes N-methylpyrrolidone.
5. The method for preparing the positive electrode slurry suitable for the battery core for electronic cigarettes according to claim 1, characterized in that: In S1, the solid content of the glue solution is 1-10%, and the viscosity is 1000-10000 mPa·s. and / or, In S5, the positive electrode slurry has a solid content of 60-80% and a viscosity of 2000-6000 mPa·s.
6. The method for preparing the positive electrode slurry suitable for the battery core for electronic cigarettes according to claim 1, characterized in that: In S4, the positive electrode active material is selected from at least one of lithium cobalt oxide materials and ternary positive electrode materials.
7. The method for preparing the positive electrode slurry suitable for the battery core for electronic cigarettes according to claim 6, characterized in that: The particle size D50 of the positive electrode active material is 5 to 10 μm, and the specific surface area is 0.1 to 0.5 m 2 / g, tap density is 2-3g / cm 3 .
8. The method for preparing the positive electrode slurry suitable for the battery core for electronic cigarettes according to claim 1, characterized in that: In S1, S2, S3 and S4, the pre-mixing operation conditions are as follows: revolution speed 5 to 50 rpm, rotation speed 50 to 500 rpm, stirring and dispersing time 5 to 50 minutes.
9. The method for preparing the positive electrode slurry suitable for the battery core for electronic cigarettes according to claim 8, characterized in that: During the stirring and dispersing operation of S1, S2, S3, S4 and S5, the reaction system is evacuated and the temperature of the reaction system is controlled to be 15-45°C.
10. A positive electrode sheet for electronic cigarette, characterized in that: The positive electrode sheet includes a positive electrode current collector and a positive electrode active coating, the positive electrode active coating is prepared from a positive electrode slurry, and the positive electrode slurry is prepared by the preparation method of a positive electrode slurry suitable for an electronic cigarette battery core according to any one of claims 1 to 9.
11. A battery cell for electronic cigarette, characterized in that: The battery core includes the positive electrode sheet for electronic cigarette as claimed in claim 10.
12. A lithium-ion battery for electronic cigarettes, characterized in that: The lithium-ion battery includes the electronic cigarette battery core as described in claim 11.
Citation Information
Cited By
Method for preparing positive electrode slurry suitable for battery cell of electronic cigarette, positive electrode sheet for electronic cigarette, battery cell, and lithium-ion battery