Selenium-doped transition metal chalcogenide thermoelectric material and preparation method thereof

By doping the transition metal chalcogenide Ta2Pd(S1-xSex)6 material, the carrier concentration and mobility are optimized, the problem of insufficient performance of existing thermoelectric materials is solved, and efficient thermoelectric performance is achieved, with environmental protection and Low cost advantage.

CN118946236APending Publication Date: 2024-11-12SHANGHAI INST OF CERAMIC CHEM & TECH CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410906498.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing thermoelectric materials such as Bi2Te3, PbTe and SiGe alloys have problems such as scarce raw materials, high toxicity, and complex preparation processes, making it difficult to develop new materials that are efficient, environmentally friendly and have high thermoelectric properties.

Method used

The selenium-doped transition metal chalcogenide Ta2Pd(S1-xSex)6 material is used to optimize the carrier concentration and mobility through doping of Se element, improve the conductivity and power factor, and enhance the thermoelectric superiority ZT.

Benefits of technology

It significantly improves the conductivity and power factor of Ta2PdS6 material, maintains the stability of the Seebeck coefficient, improves the thermoelectric superiority ZT, and has good application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946236A_ABST
    Figure CN118946236A_ABST
Patent Text Reader

Abstract

The invention relates to a selenium-doped transition metal chalcogenide thermoelectric material and a preparation method thereof. The selenium-doped transition metal chalcogenide thermoelectric material has a crystal structure represented by a composition formula of Ta2Pd (S1-xSex) 6, and x is greater than 0 and less than or equal to 0.07, preferably, x is 0.02, 0.05 or 0.07.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of inorganic thermoelectric materials, and specifically relates to a selenium-doped transition metal chalcogenide Ta2Pd (S 1-x Se x )6 Thermoelectric materials and methods for preparing the same. Background Art

[0002] Thermoelectric materials are a class of functional materials that can directly convert thermal energy into electrical energy or vice versa. With the increasing severity of the global energy crisis and environmental pollution problems, the development of efficient thermoelectric materials has become an important direction of current material science research. The performance of thermoelectric materials is usually measured by their thermoelectric figure of merit ZT, and the size of ZT depends on three parameters of the material: electrical conductivity, Seebeck coefficient and thermal conductivity. Therefore, how to optimize these parameters to improve the ZT value of the material has become the key to studying thermoelectric materials.

[0003] Among the existing thermoelectric materials, Bi2Te3, PbTe and SiGe alloys are common. However, these materials have some problems. For example, Bi2Te3 and PbTe are expensive and environmentally unfriendly due to the scarcity and toxicity of raw materials; while SiGe alloys are limited in their application due to their complex high-temperature preparation process. Therefore, the development of new, non-toxic, environmentally friendly materials with high thermoelectric performance has become an urgent need. Summary of the invention

[0004] In view of the above technical problems, the present invention aims to provide a selenium-doped transition metal chalcogenide Ta2Pd (S 1-x Se x )6 Thermoelectric materials and methods for preparing the same.

[0005] In a first aspect, the present invention provides a selenium-doped transition metal chalcogenide thermoelectric material, wherein the selenium-doped transition metal chalcogenide thermoelectric material has a composition formula of Ta2Pd(S 1-x Se x )6, wherein 0<x≤0.07, preferably x=0.02, 0.05 or 0.07.

[0006] Preferably, the crystal structure is a monoclinic, layered structure, and the layers in the layered structure are bonded by van der Waals forces; Preferably, in the crystal structure, Ta and S or Se are combined into TaS6 or TaSe6 prisms, Pd and S or Se are combined into PdS4 or PdSe4 planes, and each PdS4 or PdSe4 plane is parallel to each other.

[0007] Preferably, the conductivity of the selenium-doped transition metal chalcogenide thermoelectric material is 1 to 1000 S / cm at 300 to 700 K, the Seebeck coefficient is -100 to -200 μV / K, and the power factor is 1 to 1000 μW / mK. 2 , the dimensionless thermoelectric figure of merit ZT value is 0.01~1.

[0008] In a second aspect, the present invention provides a method for preparing the above-mentioned selenium-doped transition metal chalcogenide thermoelectric material, the preparation method comprising the following steps: (1) According to Ta2Pd(S 1-x Se x )6 stoichiometric ratio of palladium powder, sulfur powder and selenium powder are weighed to form raw material powder; (2) The raw material powder is ground and mixed, vacuum packaged, and then pre-sintered. After cooling, an ingot is obtained, and the selenium-doped transition metal chalcogenide Ta2Pd(S) is obtained by fine grinding. 1-x Se x )6 Thermoelectric powder; (3) The Ta2Pd(S 1-x Se x )6 The thermoelectric powder is sintered into a block by discharge plasma to obtain the selenium-doped transition metal sulfide compound thermoelectric material.

[0009] Preferably, in step (1), the purity of the raw material powder is 99.9%-99.999%.

[0010] Preferably, in step (2), the vacuum packaging method is plasma or flame gun packaging.

[0011] Preferably, the pre-firing temperature rise rate is 3 to 5 K / min, the pre-firing temperature is 300 to 700° C., and the pre-firing time is 12 to 72 hours.

[0012] Preferably, the fine grinding method is manual grinding or ball milling; preferably, the selenium-doped transition metal chalcogenide Ta2Pd (S 1-x Se x )6 The particle size of the thermoelectric powder is 10 to 100 μm, and the fine grinding time is 5 to 60 minutes.

[0013] Preferably, the spark plasma sintering pressure is 0.1-80 MPa, the sintering temperature is 100-600° C., and the sintering time is 0.5-120 min.

[0014] Beneficial Effects The selenium-doped transition metal chalcogenide Ta2Pd(S 1-x Se x)6 thermoelectric material and its preparation method, through the doping of Se element, the carrier concentration and mobility of Ta2PdS6 material are optimized, so that its conductivity is increased several times, the Seebeck coefficient does not decrease too much, the power factor is greatly improved, and the thermoelectric figure of merit is further enhanced, which has a good application prospect. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 The Ta2Pd(S) 1-x Se x )6 Schematic diagram of the lattice structure of selenium-doped transition metal chalcogenide thermoelectric material; Figure 2 The Ta2Pd(S) 1-x Se x )6 Schematic diagram of the preparation process of selenium-doped transition metal chalcogenide thermoelectric materials; Figure 3 The Ta2Pd(S) prepared in Example 1 of the present invention 1-x Se x )6 SEM image of selenium-doped transition metal chalcogenide thermoelectric material powder sample; Figure 4 The Ta2Pd(S) 1-x Se x ) XRD patterns of 6Se-doped transition metal chalcogenide thermoelectric materials and Ta2PdS6 powder samples; Figure 5 The Ta2Pd(S) 1-x Se x ) XRD patterns of bulk samples of 6Se-doped transition metal chalcogenide thermoelectric materials and bulk samples of Ta2PdS6; Figure 6 The Ta2Pd(S) prepared in Example 1 of the present invention 1-x Se x )6 SEM and EDS images of bulk samples of selenium-doped transition metal chalcogenide thermoelectric materials; Figure 7 The Ta2Pd(S) 1-x Se x )6 The conductivity curve of selenium-doped transition metal chalcogenide thermoelectric material and Ta2PdS6 changes with temperature; Figure 8 The Ta2Pd(S) 1-x Se x )6 The curve of Seebeck coefficient of selenium-doped transition metal chalcogenide thermoelectric material and Ta2PdS6 changing with temperature; Fig. 9 The Ta2Pd(S)1-x Se x )6 The power factor of selenium-doped transition metal chalcogenide thermoelectric materials and Ta2PdS6 varies with temperature; Fig.10 The Ta2Pd(S) 1-x Se x )6 A graph showing the total thermal conductivity of selenium-doped transition metal chalcogenide thermoelectric materials and Ta2PdS6 as a function of temperature; Fig.11 The Ta2Pd(S) 1-x Se x )6 A graph showing the change of lattice thermal conductivity of selenium-doped transition metal chalcogenide thermoelectric materials and Ta2PdS6 with temperature; Fig.12 The Ta2Pd(S) 1-x Se x )6 Selenium-doped transition metal chalcogenide thermoelectric materials and Ta2PdS6 carrier thermal conductivity versus temperature; Fig.13 The Ta2Pd(S) 1-x Se x )6The curve of the thermoelectric figure of merit (ZT) of selenium-doped transition metal chalcogenide thermoelectric materials and Ta2PdS6 changing with temperature. DETAILED DESCRIPTION

[0016] The present invention is further described below by the following embodiments. It should be understood that the following embodiments are only used to illustrate the present invention, but not to limit the present invention.

[0017] First, the present invention provides a selenium-doped transition metal chalcogenide thermoelectric material. The selenium-doped transition metal chalcogenide thermoelectric material has a composition formula of Ta2Pd(S 1-x Se x )6, wherein 0<x≤0.07, preferably x=0.02, 0.05 or 0.07. Too large a value of x will lead to the appearance of a second phase, which will cause a sharp drop in the thermoelectric performance of the material.

[0018] In some embodiments, the crystal structure is a monoclinic, layered structure, in which layers are bonded by van der Waals forces; preferably, in the crystal structure, Ta and S or Se are bonded into TaS6 or TaSe6 prisms, Pd and S or Se are bonded into PdS4 or PdSe4 planes, and each PdS4 or PdSe4 plane is parallel to each other. This special crystal structure causes the thermoelectric material to grow along the b axis to form a one-dimensional chain, and the performance of the thermoelectric material along the one-dimensional chain is the highest.

[0019] Ta2PdS6 is a layered transition metal sulfide with excellent electrical properties and thermoelectric conversion potential. The phonon scattering in the layered material of this material is strong, which can effectively reduce the lattice thermal conductivity and improve the ZT value of the material, but the electrical conductivity of Ta2PdS6 with a single component often cannot reach an ideal state. The present invention can effectively adjust the carrier concentration and mobility of the material by Se (selenium) doping, thereby improving the electrical conductivity of the material. Moreover, the radius of the Se atom is similar to that of S (sulfur), and can be doped into the lattice without significantly destroying the Ta2PdS6 lattice structure, maintaining the structural characteristics of the material. At the same time, Ta2PdSe6 is an isomorph of Ta2PdS6, with the same lattice structure, a band gap close to 0eV, and is a semi-metal with extremely high electrical conductivity. Therefore, by Se doping Ta2PdS6, the electrical transport performance can be significantly improved, which can not only enrich the thermoelectric material system, but also provide a new way to improve the performance of thermoelectric materials.

[0020] In some embodiments, the conductivity of the selenium-doped transition metal chalcogenide thermoelectric material may be 1 to 1000 S / cm at 300 to 700 K, the Seebeck coefficient may be -100 to -200 μV / K, and the power factor may be 1 to 1000 μW / mK. 2 , the dimensionless thermoelectric figure of merit (ZT value) can be 0.01 to 1; preferably, the 7% selenium-doped Ta2Pd (S 0.93 Se 0.07 )6The electrical conductivity of thermoelectric materials can reach nearly 5 times that of Ta2PdS6, and the thermoelectric power factor can reach nearly 3 times that of Ta2PdS6.

[0021] The following is an exemplary description of the preparation method of the selenium-doped transition metal chalcogenide thermoelectric material provided by the present invention. The preparation method may include the following steps: (1) According to Ta2Pd(S 1-x Se x )6 weigh tantalum powder, palladium powder, sulfur powder and selenium powder to form raw material powder; (2) The raw material powder is ground and mixed, vacuum packaged, and then pre-sintered. After cooling, an ingot is obtained, and the selenium-doped transition metal chalcogenide Ta2Pd(S) is obtained by fine grinding. 1-x Se x )6 Thermoelectric powder; (3) The Ta2Pd(S 1-x Se x )6 The thermoelectric powder is subjected to spark plasma sintering (SPS) to form a block to obtain the selenium-doped transition metal chalcogenide thermoelectric material.

[0022] In some embodiments, in step (1), the purity of the raw material powder may be 99.9%-99.999%.

[0023] In some embodiments, in step (2), the vacuum packaging method can be plasma or flame gun packaging.

[0024] In some embodiments, the pre-calcination temperature rise rate may be 3 to 5 K / min, the pre-calcination temperature may be 300 to 700° C., and the pre-calcination time may be 12 to 72 hours. The pre-calcination step may make the reaction more complete, thereby obtaining Ta2Pd(S 1-x Se x )6Pure phase of thermoelectric material.

[0025] In some embodiments, the fine grinding method can be manual grinding or ball milling; preferably, the selenium-doped transition metal chalcogenide Ta2Pd (S 1-x Se x )6 The particle size of the thermoelectric powder is 10 to 100 μm, and the fine grinding time can be 5 to 60 minutes.

[0026] In some embodiments, the SPS sintering pressure may be 0.1-80 MPa, the sintering temperature may be 100-600°C, and the sintering time may be 0.5-120 min. If the sintering pressure is too high, the sample will be broken, while if the pressure is too low, the sample will be loose; if the temperature is too low, the sample cannot be sintered to be dense, while if the temperature is too high, impurities will appear in the sample; if the sintering time is too short, the sample will be loose, while if the sintering time is too long, impurities will be generated.

[0027] The Se-doped Ta2Pd(S 1-x Se x )6 thermoelectric material and its preparation method, aiming to optimize the electrical properties of Ta2PdS6 by doping, thereby improving its thermoelectric figure of merit ZT. The method is simple and easy to implement, has the advantages of low cost, non-toxic and environmentally friendly, and can provide strong technical support for the future application of thermoelectric materials. Through systematic research on the structure, composition and performance of the material, the present invention not only provides a theoretical basis and technical means for the development of new thermoelectric materials, but also lays a foundation for the widespread application of thermoelectric technology.

[0028] The following further examples are given to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention all belong to the scope of protection of the present invention. The specific process parameters of the following examples are also only examples within a suitable range, that is, those skilled in the art can make selections within a suitable range through the description of this article, and are not limited to the specific values ​​​​exemplified below. If not specifically stated, the technical means used in the embodiments are conventional means well known to those skilled in the art.

[0029] Example 1

[0030] The selenium-doped transition metal chalcogenide thermoelectric material (Ta2Pd(S 1-x Se x )6, x=0.02) comprises the following steps: (1) According to Ta2Pd(S 0.98 Se 0.02 )6. Weigh 99.95% purity of tantalum powder, palladium powder, sulfur powder and selenium powder in stoichiometric ratio to form raw material powder; (2) The raw material powders are mixed uniformly in a mortar, and then placed in a quartz tube for vacuum packaging under the protection of an inert gas, wherein the vacuum packaging is performed by a flame gun packaging method; the quartz tube containing the mixed powder of the single substance is placed in a muffle furnace for heating, and the temperature is increased to 450° C. at a rate of 5 K / min and maintained for 12 hours, and then the temperature is increased to 700° C. at a rate of 5 K / min and maintained for 24 hours, and then cooled, and the obtained ingot is ground into powder using a mortar to obtain a selenium-doped transition metal chalcogenide Ta2Pd(S 0.98 Se 0.02 )6 Thermoelectric powder; (3) The Ta2Pd(S 0.98 Se 0.02 )6 The thermoelectric powder was subjected to SPS sintering at a pressure of 50 MPa and 600° C. for 5 min to obtain the selenium-doped transition metal chalcogenide thermoelectric material (Ta2Pd(S 1-x Se x )6, x=0.02).

[0031] Example 2

[0032] The preparation method of the selenium-doped transition metal chalcogenide thermoelectric material provided in this embodiment refers to that in Embodiment 1, the main difference being that x=0.05.

[0033] Example 3

[0034] The preparation method of the selenium-doped transition metal chalcogenide thermoelectric material provided in this embodiment refers to that in Embodiment 1, the main difference is that: x=0.07.

[0035] Comparative Example 1

[0036] The preparation method of the selenium-doped transition metal chalcogenide thermoelectric material provided in this comparative example refers to that in Example 1, the main difference is that: x=0.1.

[0037] The thermoelectric material prepared in this comparative example showed obvious impurities, resulting in a sharp decline in thermoelectric performance.

[0038] Figure 1 The Ta2Pd(S) 1-x Se x )6 Schematic diagram of the lattice structure of selenium-doped transition metal chalcogenide thermoelectric materials. Figure 1 As can be seen in (a), Ta2Pd(S 1-x Se x )6 has a monoclinic structure. After Se doping, Se replaces part of S and enters the lattice to form the doped compound Ta2Pd(S 1-x Se x )6; from Figure 1 As can be seen in (b), Ta2Pd(S 1-x Se x )6 is a layered structure; Figure 1 As can be seen in (c), Ta and S (or Se) combine to form TaS6 (or TaSe6) prisms, and Pd and S (or Se) combine to form PdS4 (or PdSe4) planes, and each PdS4 (or PdSe4) plane is parallel to each other.

[0039] Figure 2 The Ta2Pd(S) 1-x Se x )6 Schematic diagram of the preparation process of selenium-doped transition metal chalcogenide thermoelectric materials.

[0040] Figure 3 The Ta2Pd(S) prepared in Example 1 of the present invention 1-x Se x )6 SEM image of selenium-doped transition metal chalcogenide thermoelectric material powder sample. As can be seen from the image, the thermoelectric powders are all rod-shaped crystals, with a length ranging from a few microns to more than ten microns and a width of about a few hundred nanometers.

[0041] Figure 4 The Ta2Pd(S) 1-x Se x) XRD diagram of 6-selenium-doped transition metal chalcogenide thermoelectric material and Ta2PdS6 powder sample. It can be seen from the figure that the materials prepared by the present invention are all pure phases, and no other impurity peaks are found.

[0042] Figure 5 The Ta2Pd(S) 1-x Se x ) XRD patterns of bulk samples of 6-Se-doped transition metal chalcogenide thermoelectric materials and bulk samples of Ta2PdS6. As can be seen from the figure, all the samples after sintering are pure phases, without obvious second phases.

[0043] Figure 6 The Ta2Pd(S) prepared in Example 1 of the present invention 1-x Se x )6 SEM and EDS images of bulk samples of Se-doped transition metal chalcogenide thermoelectric materials. As can be seen from the figure, none of the elements are enriched, indicating that Se is doped into the lattice without producing a second phase.

[0044] Figure 7 The Ta2Pd(S) 1-x Se x )6Selenium-doped transition metal chalcogenide thermoelectric material and Ta2PdS6 conductivity curves as a function of temperature. As can be seen from the figure, the conductivity increases with the increase of doping content, and the highest conductivity is more than 4 times higher than that of the undoped one.

[0045] Figure 8 The Ta2Pd(S) 1-x Se x )6Selenium-doped transition metal chalcogenide thermoelectric material and Ta2PdS6 show the Seebeck coefficient as a function of temperature. It can be seen from the figure that the Seebeck coefficient decreases slightly with the increase of doping content.

[0046] Fig. 9 The Ta2Pd(S) 1-x Se x )6Selenium-doped transition metal chalcogenide thermoelectric material and Ta2PdS6 power factor versus temperature. As can be seen from the figure, the power factor is on the rise with the increase of doping content, and can be increased by more than 3 times.

[0047] Fig.10 The Ta2Pd(S) 1-x Se x)6Selenium-doped transition metal chalcogenide thermoelectric material and Ta2PdS6 total thermal conductivity versus temperature. It can be seen from the figure that the total thermal conductivity increases first and then decreases with the increase of doping content, and decreases with the increase of temperature.

[0048] Fig.11 The Ta2Pd(S) 1-x Se x )6Selenium-doped transition metal chalcogenide thermoelectric material and Ta2PdS6 lattice thermal conductivity versus temperature. As can be seen from the figure, the lattice thermal conductivity first increases and then decreases with the increase of doping content, and decreases with the increase of temperature.

[0049] Fig.12 The Ta2Pd(S) 1-x Se x )6Selenium-doped transition metal chalcogenide thermoelectric material and Ta2PdS6 carrier thermal conductivity versus temperature. It can be seen from the figure that the carrier thermal conductivity increases with the increase of doping content and increases with the increase of temperature.

[0050] Fig.13 The Ta2Pd(S) 1-x Se x )6Selenium doped transition metal chalcogenide thermoelectric material and Ta2PdS6 thermoelectric figure of merit (ZT) versus temperature. It can be seen from the figure that the thermoelectric figure of merit (ZT) increases with the increase of doping content and increases with the increase of temperature.

[0051] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be apparent to those skilled in the art that various modifications and substitutions of the present invention will occur. Therefore, the protection scope of the present invention should be limited by the appended claims.

Claims

1. A selenium-doped transition metal chalcogenide thermoelectric material, characterized in that: The selenium-doped transition metal chalcogenide thermoelectric material has a composition formula of Ta2Pd(S 1-x Se x )6, wherein 0<x≤0.07, preferably x=0.02, 0.05 or 0.

07.

2. The selenium-doped transition metal chalcogenide thermoelectric material according to claim 1, characterized in that: The crystal structure is a monoclinic, layered structure, in which layers are bonded by van der Waals forces; Preferably, in the crystal structure, Ta and S or Se are combined into TaS6 or TaSe6 prisms, Pd and S or Se are combined into PdS4 or PdSe4 planes, and each PdS4 or PdSe4 plane is parallel to each other.

3. The selenium-doped transition metal chalcogenide thermoelectric material according to claim 1 or 2, characterized in that: The conductivity of the selenium-doped transition metal chalcogenide thermoelectric material is 1 to 1000 S / cm at 300 to 700 K, the Seebeck coefficient is -100 to -200 μV / K, and the power factor is 1 to 1000 μW / mK. 2 , the dimensionless thermoelectric figure of merit ZT value is 0.01~1.

4. A method for preparing the selenium-doped transition metal chalcogenide thermoelectric material according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: (1) According to Ta2Pd(S 1-x Se x )6 stoichiometric ratio of palladium powder, sulfur powder and selenium powder are weighed to form raw material powder; (2) The raw material powder is ground and mixed, vacuum packaged, and then pre-sintered. After cooling, an ingot is obtained, and the selenium-doped transition metal chalcogenide Ta2Pd(S) is obtained by fine grinding. 1-x Se x )6 Thermoelectric powder; (3) The Ta2Pd(S 1-x Se x )6 The thermoelectric powder is sintered into a block by discharge plasma to obtain the selenium-doped transition metal sulfide compound thermoelectric material.

5. The preparation method according to claim 4, characterized in that: In step (1), the purity of the raw material powder is 99.9%-99.999%.

6. The preparation method according to claim 4 or 5, characterized in that: In step (2), the vacuum packaging method is plasma or flame gun packaging.

7. The preparation method according to any one of claims 4 to 6, characterized in that: The pre-burning temperature rise rate is 3-5K / min, the pre-burning temperature is 300-700°C, and the pre-burning time is 12-72 hours.

8. The preparation method according to any one of claims 4 to 7, characterized in that: The fine grinding method is manual grinding or ball milling; preferably, the selenium-doped transition metal chalcogenide Ta2Pd (S 1-x Se x )6 The particle size of the thermoelectric powder is 10 to 100 μm, and the fine grinding time is 5 to 60 minutes.

9. The preparation method according to any one of claims 4 to 8, characterized in that: The spark plasma sintering pressure is 0.1-80 MPa, the sintering temperature is 100-600° C., and the sintering time is 0.5-120 min.