Butane diisocyanate derivative, method for producing butane diisocyanate derivative, polyisocyanate composition, polyurethane resin-forming composition, coating composition, and coating film

By developing butane diisocyanate derivatives and their compositions, combined with specific manufacturing methods, the problems of high viscosity and insufficient hardness of polyisocyanate compositions in the prior art are solved, and low viscosity, excellent quick drying properties and high hardness are achieved. The coating composition reduces environmental load and energy consumption.

CN118946552APending Publication Date: 2024-11-12TOSOH CORP
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202380029545.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-27
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, the polyisocyanate composition containing isocyanurate groups has problems such as high viscosity and increased use of dilution solvents, and the polyisocyanate composition fails to fully take into account both low viscosity and high hardness.

Method used

Developed a butane diisocyanate derivative containing isocyanurate groups and urethdione groups, with a molar ratio of 20/80 to 80/20, and the weight average molecular weight of gel permeation chromatography is controlled below 790 g/mol , in combination with the method of producing a polyisocyanate composition, including a heating step and the use of an isocyanurate esterification catalyst, to form a coating film with low viscosity, excellent rapid drying properties and high hardness.

Benefits of technology

A polyisocyanate composition with low viscosity, excellent quick drying properties and high hardness is achieved, which is suitable for the preparation of high-performance coating films, reducing the amount of organic solvent used in the coating composition and the thermal energy required for the curing reaction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005054864310000061
    Figure BDA0005054864310000061
  • Figure BDA0005054864310000062
    Figure BDA0005054864310000062
  • Figure BDA0005054864310000271
    Figure BDA0005054864310000271
Patent Text Reader

Abstract

A butane diisocyanate derivative having an isocyanurate group and a uretdione group, the molar ratio of the isocyanurate group to the uretdione group being 20 / 80 to 80 / 20, and the butane diisocyanate derivative having a weight-average molecular weight of 790 g / mol or less as determined by gel permeation chromatography.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a butane diisocyanate derivative, a method for producing the butane diisocyanate derivative, a polyisocyanate composition, a polyurethane resin-forming composition, a coating composition, and a coating film. Background Art

[0002] From the perspective of reducing environmental load, the development of polyisocyanate compositions that pursue low viscosity / quick-drying properties is prevalent. By reducing the viscosity of the polyisocyanate composition, the amount of organic solvent used in the coating composition can be reduced. The excellent drying properties of the polyisocyanate composition can reduce the heat energy required for the curing reaction.

[0003] Here, Patent Document 1 discloses a covering composition, wherein an adhesive comprises (a) an isocyanurate-containing polyisocyanate and (b) a polyol component at a specified ratio, wherein the isocyanurate-containing polyisocyanate is made of 1,4-diisocyanatobutane (BDI) and has an isocyanate content of 20 to 30% by weight and a monomeric BDI content of less than 2% by weight. According to Patent Document 1, the isocyanurate-containing polyisocyanate can be rapidly dried under mild curing conditions to form a coating.

[0004] In addition, Patent Document 2 discloses a polyisocyanate composition, which contains a copolymerized polyisocyanate containing an aliphatic diisocyanate unit and an alicyclic diisocyanate unit, and / or an aliphatic polyisocyanate containing an aliphatic diisocyanate unit and an alicyclic polyisocyanate containing an alicyclic diisocyanate unit, wherein the molar ratio of the aliphatic diisocyanate unit / the alicyclic diisocyanate unit in the polyisocyanate composition is a specified ratio, and the polyisocyanate composition contains a polyisocyanate having a specified content of isocyanurate groups and has a specified viscosity. According to Patent Document 2, the polyisocyanate composition has a low viscosity and excellent quick-drying properties.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Laid-Open No. 9-132751

[0008] Patent Document 2: Japanese Patent Application Publication No. 2015-127368 Summary of the invention

[0009] Problem that the invention aims to solve

[0010] However, the isocyanurate group-containing polyisocyanate described in Patent Document 1 has problems such as high viscosity and increased amount of dilution solvent used. In addition, the polyisocyanate composition described in Patent Document 2 does not study the hardness of the resulting coating film, and the balance between low viscosity and high hardness is insufficient.

[0011] Here, in particular, in recent years, the market demand for reducing environmental load has become extremely high, but as mentioned above, it is difficult to realize a polyisocyanate composition that has low viscosity, excellent quick-drying properties, and contributes to the production of a coating film with high hardness.

[0012] Therefore, one embodiment of the present disclosure is to provide a polyisocyanate composition that has low viscosity, excellent quick-drying properties, and is helpful in producing a coating film with high hardness. Other embodiments of the present disclosure are to provide a butane diisocyanate derivative that is helpful in producing the polyisocyanate composition and a method for producing the butane diisocyanate derivative. Still other embodiments of the present disclosure are to provide a polyurethane resin-forming composition, a coating composition, and a coating film using the polyisocyanate composition.

[0013] Solutions for solving problems

[0014] The present disclosure provides the following [1] to

[11] in several aspects. [1]

[0016] A butane diisocyanate derivative having an isocyanurate group and a uretdione group,

[0017] The molar ratio of the isocyanurate group to the uretdione group is 20 / 80 to 80 / 20,

[0018] The butane diisocyanate derivative has a weight average molecular weight of 790 g / mol or less based on gel permeation chromatography. [2]

[0020] The butane diisocyanate derivative according to [1], comprising butane diisocyanate trimer and butane diisocyanate dimer,

[0021] The total content of the butane diisocyanate trimer and the butane diisocyanate dimer is 45 to 95% by mass based on the total mass of the butane diisocyanate derivative. [3]

[0023] The butane diisocyanate derivative according to [1] or [2], wherein the molar ratio of the isocyanurate group to the uretdione group is 50 / 50 or more. [4]

[0025] The butane diisocyanate derivative according to any one of [1] to [3], wherein the molar ratio of the isocyanurate group to the uretdione group is 60 / 40 or less. [5]

[0027] A method for producing a butane diisocyanate derivative according to any one of [1] to [4], comprising:

[0028] A first heating step, heating the reactant containing butane diisocyanate to above 80° C.; and

[0029] In the second heating step, the reactant that has undergone the first heating step is heated at 80 to 180° C. in the presence of an isocyanurate-forming catalyst. [6]

[0031] The method for producing a butane diisocyanate derivative according to [5], wherein the isocyanuration catalyst comprises an aminosilyl group-containing compound. [7]

[0033] A polyisocyanate composition comprising the butane diisocyanate derivative according to any one of [1] to [4]. [8]

[0035] The polyisocyanate composition according to [7], wherein the viscosity at 25° C. is 2500 mPa·s or less. [9]

[0037] A polyurethane resin-forming composition comprising the polyisocyanate composition described in [7] or [8] and a polyol.

[10]

[0039] A coating composition comprising the polyisocyanate composition described in [8] and a compound having two or more isocyanate-reactive groups.

[11]

[0041] A coating film comprising a cured product of the coating composition described in

[10] .

[0042] Effects of the Invention

[0043] According to one embodiment of the present disclosure, a polyisocyanate composition having low viscosity, excellent quick-drying property, and helpful for producing a coating film having high hardness can be provided. According to other embodiments of the present disclosure, a butane diisocyanate derivative that is helpful for producing the polyisocyanate composition and a method for producing the butane diisocyanate derivative can be provided. According to still other embodiments of the present disclosure, a polyurethane resin-forming composition, a coating composition, and a coating film using the polyisocyanate composition can be provided. DETAILED DESCRIPTION

[0044] In this specification, the numerical range represented by "~" represents a range including the numerical values ​​recorded before and after "~" as the minimum and maximum values, respectively. In the numerical range recorded in stages in this specification, the upper limit or lower limit of the numerical range of a certain stage can also be replaced by the upper limit or lower limit of the numerical range of other stages. In addition, in the numerical range recorded in this specification, the upper limit or lower limit of the numerical range can also be replaced by the value shown in the embodiment. In addition, the upper limit and lower limit recorded separately can be combined arbitrarily.

[0045] Hereinafter, preferred embodiments of each aspect of the present disclosure will be described. However, each aspect of the present disclosure is not limited to the following embodiments at all.

[0046] <Butane diisocyanate derivative and polyisocyanate composition>

[0047] The butane diisocyanate derivative of one embodiment of the present disclosure has an isocyanurate group and a uretdione group, the molar ratio of the isocyanurate group to the uretdione group (total molar number of isocyanurate groups / total molar number of uretdione groups) is 20 / 80 to 80 / 20, and the weight average molecular weight based on gel permeation chromatography is 790 g / mol or less. In the following description, butane diisocyanate is sometimes referred to as "BDI", and the molar ratio of the isocyanurate group to the uretdione group is sometimes referred to as "molar ratio (I / U)".

[0048] According to the above-mentioned BDI derivative, a polyisocyanate composition having low viscosity and excellent quick-drying property and being helpful in preparing a coating film with high hardness can be prepared. It should be noted that the low viscosity of the polyisocyanate composition can be confirmed, for example, by the viscosity at 25°C measured by a rheometer. In addition, the excellent quick-drying property of the polyisocyanate composition can be confirmed, for example, by the curing start temperature of the coating film formed by the coating composition prepared using the polyisocyanate composition. In addition, the coating film obtained using the polyisocyanate composition has high hardness, for example, by the Martens hardness of the coating film at 23°C.

[0049] The polyisocyanate composition of another embodiment of the present disclosure comprises a BDI derivative having an isocyanurate group and a uretdione group at a molar ratio (I / U) of 20 / 80 to 80 / 20. The weight average molecular weight of the BDI derivative based on gel permeation chromatography is preferably 790 g / mol or less. That is, the BDI derivative is preferably the above-mentioned BDI derivative.

[0050] The polyisocyanate composition has a tendency to have low viscosity and excellent quick-drying properties. Furthermore, the polyisocyanate composition can easily form a coating film having high hardness.

[0051] BDI derivatives are mixtures of various compounds derived from BDI monomers. BDI derivatives include, for example, isocyanurate forms of BDI and uretdione forms of BDI. The isocyanurate form of BDI is a compound having an isocyanurate group (a group formed by cyclopolymerization of 3 molecules of BDI monomer) in a compound derived from a BDI monomer. The uretdione form of BDI is a compound having a uretdione group (a group formed by cyclopolymerization of 2 molecules of BDI monomer) in a compound derived from a BDI monomer. BDI derivatives may include compounds having an isocyanurate group and a uretdione group (a compound that is an isocyanurate form and also a uretdione form) in a compound derived from a BDI monomer. Such compounds are equivalent to both the isocyanurate form of BDI and the uretdione form of BDI.

[0052] BDI monomers as raw materials of BDI isocyanurate and BDI uretdione include, for example, 1,2-butane diisocyanate, 1,3-butane diisocyanate, 1,4-butane diisocyanate, 2,3-butane diisocyanate, and mixtures thereof. From the perspective of high reactivity of isocyanate groups bonded to primary carbons, the raw materials of BDI isocyanurate and BDI uretdione preferably include 1,4-butane diisocyanate. The proportion of 1,4-butane diisocyanate in the raw materials of BDI isocyanurate and the proportion of 1,4-butane diisocyanate in the raw materials of BDI uretdione can be 90% by mass or more, 95% by mass or more, or 100% by mass. Below, the method of using 1,4-butane diisocyanate as a BDI monomer is described as an example, but there is no limitation thereto unless otherwise specified.

[0053] The isocyanurate form of BDI preferably includes an isocyanurate trimer of BDI. The isocyanurate trimer of BDI is, for example, a compound represented by the following formula (1).

[0054]

[0055] The isocyanurate of BDI may include a tetramer or more polymer formed by the reaction and polymerization of the isocyanate group (hereinafter sometimes referred to as "NCO group") in the isocyanurate trimer of BDI with the NCO group in other BDI monomers (or compounds derived from other BDI monomers). The isocyanurate of BDI more preferably includes the isocyanurate trimer of BDI and the above-mentioned tetramer or more polymers, and further preferably includes the isocyanurate trimer of BDI, the isocyanurate pentamer of BDI (a compound formed by cyclopolymerization of one NCO group in the isocyanurate trimer of BDI with two molecules of other BDI monomers), and the isocyanurate heptamer of BDI (a compound formed by cyclopolymerization of two NCO groups in the isocyanurate trimer of BDI with two molecules of other BDI monomers, respectively). As described above, the isocyanurate of BDI may contain a compound having a uretdione group (for example, a compound in which one or two NCO groups in the isocyanurate trimer of BDI are cyclopolymerized with one molecule of another BDI monomer) as the above-mentioned tetramer or higher polymer.

[0056] The uretdione form of BDI preferably includes a uretdione dimer of BDI. The uretdione dimer of BDI is, for example, a compound represented by the following formula (2).

[0057]

[0058] The uretdione form of BDI may also include a trimer or more polymer formed by further reacting and polymerizing the NCO group in the uretdione dimer of BDI with the NCO group in other BDI monomers (or compounds derived from other BDI monomers). The uretdione form of BDI more preferably includes the uretdione dimer of BDI and the above-mentioned trimer or more polymers, and further preferably includes the uretdione dimer of BDI, the uretdione trimer of BDI (a compound formed by cyclization polymerization of one NCO group in the uretdione dimer of BDI with one molecule of other BDI monomers), and the uretdione tetramer of BDI (a compound formed by cyclization polymerization of two NCO groups in the uretdione dimer of BDI with one molecule of other BDI monomers, respectively). As described above, the uretdione form of BDI may contain a compound having an isocyanurate group (for example, a compound in which one or two NCO groups in the uretdione dimer of BDI are cyclopolymerized with two other BDI monomer molecules) as the above-mentioned trimer or higher polymer.

[0059] BDI derivatives have a molar ratio (I / U). The molar ratio (I / U) is the molar ratio of the isocyanurate group to the uretdione group in the BDI derivative, which can be renamed as the molar ratio of the isocyanurate group of the isocyanurate body of BDI to the uretdione group of the uretdione body of BDI. The molar ratio (I / U) of the BDI derivative is 20 / 80 to 80 / 20, and can be 25 / 75 or more, 30 / 70 or more, or 50 / 50 or more, or 75 / 25 or less, 70 / 30 or less, or 60 / 40 or less. When the molar ratio (I / U) is 50 / 50 or more, there is a tendency to obtain a coating film with higher hardness, and when the molar ratio (I / U) is 60 / 40 or less, there is a tendency to further reduce the viscosity. The molar ratio (I / U) can be measured, for example, by using a nuclear magnetic resonance device (NMR). 1 H-NMR method measurement. More specifically, it can be measured according to the examples described below.

[0060] The BDI derivative and the polyisocyanate composition preferably contain BDI trimers (eg, BDI isocyanurate trimers and BDI uretdione trimers) and BDI dimers (eg, BDI uretdione dimers). In this case, the viscosity of the polyisocyanate composition tends to be lower, and workability tends to be better.

[0061] From the viewpoint of promoting the low viscosity of the polyisocyanate composition, the total content of BDI trimer and BDI dimer is preferably 45% by mass or more, more preferably 50% by mass or more, and further preferably 55% by mass or more. From the viewpoint of increasing the crosslinking density of the resin, the total content of BDI trimer and BDI dimer is preferably 95% by mass or less, more preferably 90% by mass or less, and further preferably 85% by mass or less. From these viewpoints, the total content of BDI trimer and BDI dimer can be, for example, 45 to 95% by mass. The total content of BDI trimer and BDI dimer can also be 60% by mass or more, 65% by mass or more, 75% by mass or more, or 80% by mass or less, 75% by mass or less, 70% by mass or less, or 65% by mass or less.

[0062] From the viewpoint of promoting high hardness of the coating film, the content of the BDI trimer may be 20% by mass or more, or 30% by mass or more, 35% by mass or more, or 40% by mass or more. From the viewpoint of promoting low viscosity of the polyisocyanate composition, the content of the BDI trimer may be 90% by mass or less, or 65% by mass or less, 55% by mass or less, or 45% by mass or less. From these viewpoints, the content of the BDI trimer may be, for example, 20 to 90% by mass, or 20 to 65% by mass.

[0063] From the viewpoint of promoting the low viscosity of the polyisocyanate composition, the content of BDI dimer may be 10% by mass or more, or 15% by mass or more, 20% by mass or more, or 35% by mass or more. From the viewpoint of promoting the high hardness of the coating film, the content of BDI dimer may be 80% by mass or less, or 65% by mass or less, 50% by mass or less, or 40% by mass or less. From these viewpoints, the content of BDI dimer may be, for example, 10 to 80% by mass, or 10 to 65% by mass.

[0064] The total content of BDI trimer and BDI dimer, and the content of each of BDI trimer and BDI dimer are based on the total mass of the BDI derivative or the total mass of the solid content in the polyisocyanate composition, and are values ​​calculated from the differential refractive index peak of the BDI derivative or the polyisocyanate composition based on gel permeation chromatography (GPC). More specifically, these amounts can be measured according to the Examples described below.

[0065] The BDI derivative and the polyisocyanate composition may further contain a compound derived from a BDI monomer (e.g., a biuret form of BDI, etc.) in addition to the isocyanurate form of BDI and the uretdione form of BDI, and the content of the compound (hereinafter also referred to as "other BDI derivatives") is preferably 20 mol% or less, more preferably 1 mol% or less (the above compound is substantially not contained). The above content is based on the total number of moles of the isocyanurate group, uretdione group and other BDI derivatives (e.g., the biuret form of BDI, etc.) in the BDI derivative.

[0066] From the viewpoint of increasing the NCO groups used in the crosslinking of the polyurethane resin, the NCO content of the BDI derivative may be 10% by mass or more, 20% by mass or more, or 25% by mass or more, based on the total mass of the solid content in the polyisocyanate composition. From the viewpoint of reducing the content of low molecular weight components such as BDI monomer in order to suppress odor, the NCO content of the BDI derivative may be 36% by mass or less, 33% by mass or less, or 30% by mass or less, based on the total mass of the solid content in the polyisocyanate composition. From these viewpoints, the NCO content of the BDI derivative may be, for example, 10 to 36% by mass, based on the total mass of the solid content in the polyisocyanate composition.

[0067] In order to extend the pot life and make the coating composition one-component, the BDI derivative can be blocked with a known blocking agent. That is, part or all of the NCO groups in the isocyanurate body of BDI can be blocked with a blocking agent, and part or all of the NCO groups in the uretdione body of BDI can be blocked with a blocking agent. The blocked polyisocyanate is inactive at room temperature, but by heating, the blocking agent decomposes, and the isocyanate group is activated again, thereby reacting with the active hydrogen group. The blocking agent is a compound having one active hydrogen in the molecule, for example, alcohols, alkylphenols, phenols, active methylene, thiol, amide, imide, imidazole, urea, oxime, amine, imide, pyrazole and other known blocking agents can be used. It should be noted that when the BDI derivative is blocked, the weight average molecular weight and viscosity described later are measured after the blocking agent is decomposed.

[0068] The weight average molecular weight of the BDI derivative based on gel permeation chromatography (GPC) is 790g / mol or less, preferably 750g / mol or less, and more preferably 710g / mol or less. By making the weight average molecular weight of the BDI derivative within the above range, a polyisocyanate composition having good compatibility with the main agent and low viscosity can be obtained. The above weight average molecular weight may also be 690g / mol or less, 650g / mol or less, 600g / mol or less, or 550g / mol or less. From the perspective of promoting the high hardness of the coating film, the above weight average molecular weight may be 400g / mol or more, or 450g / mol or more, 500g / mol or more, 550g / mol or more, or 600g / mol or more. From the same point of view, the weight average molecular weight of the polyisocyanate composition based on gel permeation chromatography may also be within the above range. The above weight average molecular weight may be more specifically measured according to the embodiments described below.

[0069] The polyisocyanate composition may contain other components in addition to the BDI derivative, or may contain only the BDI derivative. Examples of other components include 1,1-hexane diisocyanate (hereinafter sometimes referred to as "HDI") and its derivatives.

[0070] The polyisocyanate composition may contain isocyanate compounds other than BDI derivatives (e.g., polyisocyanates such as BDI monomer, HDI monomer, and HDI derivatives) as other components, and the content of BDI monomer in the polyisocyanate composition is preferably 5% by mass or less, more preferably 1% by mass or less (substantially no BDI monomer is contained). In addition, the content of isocyanate compounds other than BDI derivatives in the polyisocyanate composition is preferably 50% by mass or less, more preferably 1% by mass or less (substantially no isocyanate compounds other than BDI derivatives are contained). The above content is based on the total mass of the solid content in the polyisocyanate composition.

[0071] The polyisocyanate composition may contain the organic solvents described below as other components. The content of the organic solvent in the polyisocyanate composition is preferably 50% by mass or less, more preferably 20% by mass or less (substantially free of organic solvents). The above content is based on the total mass of the solid components in the polyisocyanate composition.

[0072] The viscosity of the polyisocyanate composition at 25°C is preferably 3000 mPa·s or less, more preferably 2500 mPa·s or less, further preferably 2000 mPa·s or less, still further preferably 1000 mPa·s or less, and particularly preferably 500 mPa·s or less. When the above viscosity is 2500 mPa·s or less, the polyisocyanate composition has good workability even without being diluted with a large amount of solvent, and the solid component concentration of the coating composition can be further increased. The viscosity of the polyisocyanate composition at 25°C can be, for example, 50 mPa·s or more, can be 100 mPa·s or more, or can be 150 mPa·s or more. When the viscosity is 50 mPa·s or more, the resulting coating film tends to have higher hardness. From the aspect of easily obtaining the polyisocyanate composition with the above viscosity, the preferred range of the viscosity of the BDI derivative at 25°C is the same as the above range.

[0073] The BDI derivative and the polyisocyanate composition described above are suitable as a curing agent component for a coating composition. That is, another embodiment of the present disclosure is a coating curing agent containing the above BDI derivative, and still another embodiment of the present disclosure is a coating curing agent containing the above polyisocyanate composition. It should be noted that as the main agent for these coating curing agents, the isocyanate-reactive compounds (polyols, etc.) described below can be used.

[0074] <Manufacturing method of BDI derivative>

[0075] Another aspect of the present disclosure is a method for manufacturing the BDI derivative of the above embodiment. The manufacturing method of the BDI derivative includes a polymerization step of obtaining a polymer of BDI (isocyanurate form of BDI and uretidione form of BDI) by performing an isocyanuration reaction for forming an isocyanurate group and a uretidionation reaction for forming a uretidione group.

[0076] The isocyanuration reaction can be carried out, for example, in the presence of a generally known isocyanuration catalyst. Examples of the isocyanuration catalyst include quaternary ammonium salts, metal carboxylates, and silylamine-containing compounds. The isocyanuration catalyst can be used alone or in combination of two or more.

[0077] As the isocyanuration catalyst, from the viewpoint of suppressing the formation of high molecular weight bodies, aminosilyl group-containing compounds such as aminosilane and silylurea are preferably used, disilazanes such as hexamethyldisilazane and heptamethyldisilazane are more preferably used, and hexamethyldisilazane is further preferably used.

[0078] The amount of the isocyanuration catalyst used is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of the BDI input. The larger the amount of the isocyanuration catalyst used, the greater the molar ratio (I / U) is likely to be.

[0079] The reaction temperature of the isocyanurate reaction is preferably 80 to 180° C., more preferably 100 to 160° C. When the reaction temperature of the isocyanurate reaction is 80° C. or higher, the reaction time can be shortened, so the coloring of the polyisocyanate composition can be further suppressed. In addition, when the reaction temperature of the isocyanurate reaction is 80 to 180° C., it is easy to adjust the molar ratio (I / U) to 20 / 80 to 80 / 20.

[0080] The isocyanurate reaction can be stopped by adding a reaction terminator when the target isocyanate group content and molecular weight are reached. When the reaction temperature of the isocyanurate reaction is 80 to 180° C., the reaction time of the isocyanurate reaction is, for example, 1 to 5 hours.

[0081] The reaction terminator is a compound that has the effect of deactivating the catalyst. As the reaction terminator, for example, water, a compound having a hydroxyl group, etc. can be used. The reaction terminator is preferably an alcohol. The reaction terminator can be used alone or in combination of two or more. It should be noted that the reaction terminator is preferably added quickly after reaching the target isocyanate content and molecular weight.

[0082] The amount of the reaction terminator added varies depending on the type of the reaction terminator, the type of the isocyanurate catalyst used, etc., and is preferably 0.1 to 3.5 equivalents, particularly preferably 0.8 to 2.5 equivalents, relative to 1 equivalent of the isocyanurate catalyst. When the amount of the reaction terminator used is 0.1 equivalent or more relative to 1 equivalent of the isocyanurate catalyst, the storage stability of the obtained polyisocyanate composition becomes better. When the amount of the reaction terminator used is 3.5 equivalents or less relative to 1 equivalent of the isocyanurate catalyst, the formation of the reaction product of the reaction terminator and BDI can be suppressed, and thus the reduction of the isocyanate group content can be more highly suppressed.

[0083] The uretdione reaction can be carried out in the presence of a generally known uretdione catalyst, for example, tertiary phosphines such as trialkylphosphine and tribenzylphosphine, and Lewis acids such as boron trifluoride and zinc trichloride.

[0084] When a uretdione catalyst is used, the uretdione reaction can be stopped by adding phosphoric acid, methyl p-toluenesulfonate or the like when the molar ratio (I / U) reaches a desired ratio.

[0085] The uretdione reaction can also be carried out by heating the reactant (e.g., BDI monomer) without using the uretdione reaction catalyst as described above. From the viewpoint of suppressing the generation of by-products, it is preferred to carry out the uretdione reaction only by heating without using a uretdione reaction catalyst. The heating temperature is preferably 80° C. or more, more preferably 100 to 170° C., and further preferably 110 to 160° C. When the heating temperature is 80 to 170° C., it is easy to suppress the generation of by-products and adjust the molar ratio (I / U) to 20 / 80 to 80 / 20.

[0086] The isocyanurate conversion reaction and the uretdione conversion reaction can be carried out under an inert gas atmosphere such as nitrogen or argon. Specifically, BDI can be introduced into a reaction container, and an inert gas such as nitrogen or argon can be introduced into the container to make the reaction atmosphere an inert gas atmosphere, and then the isocyanurate conversion reaction and the uretdione conversion reaction can be carried out by the above method.

[0087] Isocyanurate reaction and uretdione reaction can be carried out in the absence of organic solvent, or in the presence of organic solvent. When reacting in the presence of organic solvent, it is preferred to use an organic solvent that will not affect the reaction and has a boiling point above the reaction temperature. As organic solvent, ketones such as aliphatic hydrocarbons such as octane, alicyclic hydrocarbons such as cyclohexane and methylcyclohexane, methyl isobutyl ketone, cyclohexanone, butyl acetate, esters such as isobutyl acetate, ethylene glycol ether acetate, propylene glycol monomethyl ether acetate, 3-methyl-3-methoxybutyl acetate, glycol ether esters such as ethyl-3-ethoxy propionate, ethers such as dioxane, halogenated hydrocarbons such as diiodomethane and monochlorobenzene, N-methylpyrrolidone, dimethylformamide, dimethylacetamide, dimethyl sulfoxide, hexamethylphosphamide, etc. polar aprotic solvents, etc. can be listed. Organic solvent can be used alone or in combination of two or more.

[0088] Isocyanurate reaction and uretdionization reaction can be carried out respectively in sequence, or simultaneously. In the case of carrying out isocyanurate reaction and uretdionization reaction simultaneously, the timing of reaction start and reaction stop can also be different at the same time. For example, after the uretdionization reaction of BDI can be started and the uretdionization of BDI is carried out, the reactant of the uretdion body comprising BDI is carried out uretdionization reaction and isocyanurate reaction. In the polymerization process, it is preferred to carry out isocyanurate reaction and uretdionization reaction simultaneously. In the polymerization process, it is more preferred to carry out isocyanurate reaction and stopped reaction after the uretdionization reaction utilizing heat (after the reaction starts). If the uretdionization reaction utilizing heat is carried out after the stopped reaction of isocyanurate reaction, the side reaction of the catalyst decomposition product and isocyanate generated by the side when the stopped reaction is promoted, and sometimes thickening, the reduction of isocyanate group content, etc., are occurred, so it is preferred not to carry out uretdionization reaction after the stopped reaction of isocyanurate reaction.

[0089] More specifically, the polymerization step is preferably a step including the following steps: a first heating step of heating a reactant containing BDI (BDI monomer) to 80°C or higher; and a second heating step of heating the reactant after the first heating step at 80 to 180°C in the presence of an isocyanurate catalyst. In this method, at least the uretdione reaction of BDI is carried out in the first heating step, and the isocyanurate reaction of a reactant containing a uretdione form of BDI (for example, a mixture of unreacted BDI monomer and a uretdione form of BDI) is carried out in the second heating step. The heating conditions of the first heating step are the same as the preferred range of the heating temperature of the uretdione reaction, and the heating conditions of the second heating step are the same as the preferred range of the reaction temperature of the isocyanurate reaction. It should be noted that in the second heating step, the uretdione reaction can be carried out simultaneously with the isocyanurate reaction.

[0090] From the viewpoint of increasing the amount of uretdione, the first heating step may be a step of heating the reactants to 80°C or higher and then maintaining the reactants at a temperature of 80°C or higher. The preferred range of the maintaining temperature is the same as the heating temperature of the uretdione reaction. The maintaining time is preferably 1 to 6 hours, more preferably 2 to 5 hours.

[0091] After the reaction is completed, the unreacted BDI monomer (free BDI) can be removed from the reaction solution containing the reaction product. That is, the method for producing a BDI derivative may further include a BDI removal step for removing free BDI after the polymerization step. In order to remove free BDI, for example, a removal method using thin film distillation at a high vacuum of 10 to 100 Pa and 90 to 130°C; an extraction method using an organic solvent, etc. are used. The above removal is preferably carried out in a manner such that the residual content of free BDI present in the reaction solution is 5% by mass or less. When the residual content of free BDI is 5% by mass or less, the generation of odor can be further suppressed, and the reduction in storage stability can be further suppressed. It should be noted that when an organic solvent is used in the above reaction, the organic solvent can be removed simultaneously with the removal of the above free BDI.

[0092] The method for producing a BDI derivative may further include a step of capping the BDI derivative with the above-mentioned capping agent after the polymerization step or the BDI removal step.

[0093] The BDI derivative (or the reaction solution containing the BDI derivative) obtained by the above method can be used as a polyisocyanate composition directly or after being mixed with the above other components. By mixing the polyisocyanate composition obtained in this way with a polyol, a polyurethane resin-forming composition according to one embodiment of the present disclosure can be obtained.

[0094] <Polyurethane resin forming composition>

[0095] A polyurethane resin-forming composition according to one embodiment of the present disclosure comprises the polyisocyanate composition of the above embodiment and a polyol. The composition has polyurethane resin-forming properties, and a polyisocyanate (e.g., a BDI derivative) in the composition reacts with a polyol to form a polyurethane resin as a reaction product of the polyisocyanate and the polyol.

[0096] Polyol is a compound having two or more hydroxyl groups as active hydrogen groups as reaction groups with isocyanate groups. As polyol, there is no particular limitation, and preferably polyester polyol, polyether polyol, polycarbonate polyol, polyolefin polyol, acrylic polyol, silicone polyol, castor oil polyol, fluorine polyol, ester exchange products of two or more polyols, hydroxyl-terminated prepolymers that have been subjected to urethanization reaction with polyisocyanates, etc. are used. Polyol can be used alone or in combination of two or more.

[0097] (Polyester polyol)

[0098] Examples of the polyester polyol include polyester polyols obtained by polycondensation reaction of one or more dicarboxylic acids or their anhydrides and one or more low molecular weight polyols having a molecular weight of 500 or less. Examples of the dicarboxylic acid include phthalic acid, isophthalic acid, terephthalic acid, naphthalene dicarboxylic acid, succinic acid, tartaric acid, oxalic acid, malonic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, glutaconic acid, azelaic acid, sebacic acid, 1,4-cyclohexyl dicarboxylic acid, α-hydrogenated muconic acid, β-hydrogenated muconic acid, α-butyl-α-ethylglutaric acid, α,β-diethylsuccinic acid, maleic acid, and fumaric acid. Examples of the low molecular weight polyols having a molecular weight of 500 or less include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 3-methyl-1,5-pentanediol, 3,3-dimethylolheptane, diethylene glycol, dipropylene glycol, neopentyl glycol, cyclohexane-1,4-diol, cyclohexane-1,4-dimethanol, dimer alcohol, bisphenol A, ethylene oxide or propylene oxide adducts of bisphenol A, bis(β-hydroxyethyl)benzene, benzyl alcohol, glycerin, trimethylolpropane, and pentaerythritol. In addition, lactone polyester polyols obtained by ring-opening polymerization of cyclic ester (so-called lactone) monomers such as ε-caprolactone, alkyl-substituted ε-caprolactone, δ-valerolactone, alkyl-substituted δ-valerolactone, etc. can also be used. Furthermore, polyester-amide polyols obtained by replacing part of the low molecular weight polyol with low molecular weight polyamines such as hexamethylenediamine, isophoronediamine, monoethanolamine, or low molecular weight amino alcohols can also be used.

[0099] (Polyether polyol)

[0100] As polyether polyols, for example, compounds having two or more, preferably 2 to 3 active hydrogen groups, such as low molecular weight polyols and low molecular weight polyamines, can be cited as initiators, and polyether polyols obtained by addition polymerization of alkylene oxides. As low molecular weight polyols, the same compounds as those exemplified as the above-mentioned low molecular weight polyols with a molecular weight of less than 500 can be cited. As low molecular weight polyamines, for example, ethylenediamine, propylenediamine, toluenediamine, metaphenylenediamine, diphenylmethanediamine, and xylylenediamine can be cited. As alkylene oxides, for example, ethylene oxide, propylene oxide, and butylene oxide can be cited. In addition, polyether polyols obtained by ring-opening polymerization of alkyl glycidyl ethers such as methyl glycidyl ether, aryl glycidyl ethers such as phenyl glycidyl ether, and cyclic ether monomers such as tetrahydrofuran can also be used.

[0101] (Polycarbonate polyol)

[0102] As polycarbonate polyol, for example, polycarbonate polyol obtained by dealcoholization reaction or dephenolization reaction of more than one low molecular polyol and diaryl carbonate can be listed. As low molecular polyol, the same material as the compound illustrated as the low molecular polyol of the molecular weight below 500 can be illustrated. As diaryl carbonate, for example, dialkyl carbonates such as dimethyl carbonate, diethyl carbonate, alkylene carbonates such as ethylene carbonate, propylene carbonate, diphenyl carbonate, dinaphthyl carbonate, dianthryl carbonate, diphenanthryl carbonate, diindan carbonate, tetralin carbonate etc. can be listed. In addition, as polycarbonate polyol, the polyol obtained by the transesterification reaction of polycarbonate polyol, polyester polyol and low molecular polyol can also be used.

[0103] (Polyolefin polyol)

[0104] Examples of the polyolefin polyol include polybutadiene, hydrogenated polybutadiene, polyisoprene, and hydrogenated polyisoprene having two or more hydroxyl groups.

[0105] (Acrylic polyol)

[0106] Examples of acrylic polyols include those obtained by using acrylic acid esters and / or methacrylic acid esters (hereinafter referred to as (meth)acrylic acid esters), acrylic acid hydroxy compounds and / or methacrylic acid hydroxy compounds (hereinafter referred to as (meth)acrylic acid hydroxy compounds) and a polymerization initiator, and polymerizing or copolymerizing the (meth)acrylic acid esters and / or (meth)acrylic acid hydroxy compounds using light energy such as ultraviolet rays or electron beams or heat energy.

[0107] [(Meth)acrylate]

[0108] Examples of the (meth)acrylate include alkyl esters having 1 to 20 carbon atoms. Examples of such (meth)acrylate include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, and dodecyl (meth)acrylate; esters of (meth)acrylic acid and alicyclic alcohols such as cyclohexyl (meth)acrylate; and aryl (meth)acrylates such as phenyl (meth)acrylate and benzyl (meth)acrylate. The (meth)acrylate may be used alone or in combination of two or more.

[0109] [(Meth)acrylic acid hydroxy compound]

[0110] The (meth)acrylic acid hydroxy compound has at least one hydroxyl group that can become a reaction point with polyisocyanate in the molecule. Examples of the (meth)acrylic acid hydroxy compound include acrylic acid hydroxy compounds such as 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 4-hydroxybutyl acrylate, 3-hydroxy-2,2-dimethylpropyl acrylate, and pentaerythritol triacrylate. In addition, methacrylic acid hydroxy compounds such as 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 4-hydroxybutyl methacrylate, 3-hydroxy-2,2-dimethylpropyl methacrylate, and pentaerythritol trimethacrylate can also be used. The (meth)acrylic acid hydroxy compound can be used alone or in combination of two or more.

[0111] (Silicone Polyol)

[0112] Examples of the silicone polyol include vinyl-containing silicone compounds obtained by polymerizing γ-methacryloxypropyltrimethoxysilane and the like, and polysiloxanes such as α,ω-dihydroxypolydimethylsiloxane and α,ω-dihydroxypolydiphenylsiloxane having at least one terminal hydroxyl group in the molecule.

[0113] (Castor oil based polyol)

[0114] Examples of castor oil-based polyols include linear or branched polyester polyols obtained by reacting castor oil fatty acids with polyols, dehydrated castor oil, partially dehydrated castor oil, and hydrogenated castor oil to which hydrogen is added.

[0115] (Fluorinated polyol)

[0116] As fluorine-based polyols, linear or branched polyols obtained by copolymerization of a fluorine-containing monomer as an essential component and a monomer having a hydroxyl group can be cited. Here, the fluorine-containing monomer is preferably a fluoroolefin. As fluorine-containing monomers, for example, tetrafluoroethylene, trifluorochloroethylene, trichlorofluoroethylene, hexafluoropropylene, vinylidene fluoride, vinyl fluoride, trifluoromethyltrifluoroethylene, etc. can be cited. In addition, as monomers having a hydroxyl group, for example, hydroxyalkyl vinyl ethers such as hydroxyethyl vinyl ether, 4-hydroxybutyl vinyl ether, cyclohexanediol monovinyl ether, hydroxyalkyl allyl ethers such as 2-hydroxyethyl allyl ether, hydroxyalkyl crotonate, etc., hydroxyl-containing carboxylic acid vinyl esters, hydroxyl-containing allyl esters, etc. can be cited.

[0117] The number of active hydrogen groups (average number of functional groups) in one molecule of the polyol is preferably 1.9 to 6.0. When the number of active hydrogen groups is within the above range, the resulting coating film tends to exhibit more excellent hardness.

[0118] The number average molecular weight of the polyol is preferably in the range of 750 to 50000. When the number average molecular weight of the polyol is above the lower limit, there is a tendency for the adhesion to be further improved. When the number average molecular weight of the polyol is below the upper limit, there is a tendency for the solubility in low-polarity organic solvents to be further improved and the adhesion to be further improved.

[0119] In the polyurethane resin forming composition, the content ratio of the polyisocyanate composition to the polyol is not particularly limited, and the molar ratio R (isocyanate group / hydroxyl group) of the isocyanate group in the polyisocyanate composition to the hydroxyl group in the polyol is preferably 0.5 to 2.5. When the molar ratio R is above the above lower limit, the hydroxyl group does not become excessive, so there is a tendency for the adhesion to be further improved, and the reduction in crosslinking density is suppressed, and the durability and mechanical strength of the coating film tend to become better. When the molar ratio R is below the above upper limit, the isocyanate group does not become excessive, and the reaction with moisture in the air is suppressed, so the expansion of the coating film is further reduced, and there is a tendency for the reduction in adhesion associated with this to be further suppressed.

[0120] The polyurethane resin forming composition may be a one-component composition in which all components are contained in a single component, or a multi-component composition in which components are separated into a plurality of components. For example, a multi-component composition may include a first component (main component) containing a polyol and a second component (curing agent) containing a polyisocyanate composition.

[0121] The polyurethane resin forming composition may contain a diluent solvent. When the polyurethane resin forming composition is a multi-component type, the diluent solvent may be contained in one of the first component and the second component mentioned above, or may be contained in both. The diluent solvent is, for example, an organic solvent. As the diluent solvent, for example, ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, esters such as ethyl acetate, butyl acetate, and cellosolve acetate, alcohols such as butanol and isopropanol, toluene, xylene, cyclohexane, mineral spirits, naphtha, and the like may be cited. The diluent solvent may be appropriately selected for use according to the purpose and application. The diluent solvent may be used alone or in combination of two or more.

[0122] The polyurethane resin forming composition may contain a urethanization catalyst. As the urethanization catalyst, a known urethanization catalyst may be appropriately used in consideration of the pot life, curing conditions, and operating conditions. Specific urethanization catalysts include, for example, organic metal compounds such as dibutyltin diacetate, dibutyltin dilaurate, and dioctyltin dilaurate, and organic amines such as triethylenediamine and triethylamine, or salts thereof. The urethanization catalyst may be used alone or in combination of two or more.

[0123] The polyurethane resin forming composition may be appropriately blended with additives such as antioxidants such as 2,6-di-tert-butyl-4-methylphenol, ultraviolet absorbers, pigments, dyes, solvents, flame retardants, hydrolysis inhibitors, lubricants, plasticizers, fillers, antistatic agents, dispersants, catalysts, storage stabilizers, surfactants, and leveling agents as needed. When the polyurethane resin forming composition is a multi-component type, these additives may be contained in one of the first component and the second component, or in both.

[0124] The polyurethane resin-forming composition can be suitably used as a coating composition.

[0125] <Coating composition and coating film>

[0126] A coating composition according to one embodiment of the present disclosure includes the polyisocyanate composition of the above embodiment and a compound having two or more isocyanate-reactive groups (hereinafter referred to as an isocyanate-reactive compound). In addition, a coating film according to one embodiment of the present disclosure includes a cured product of the above coating composition.

[0127] The isocyanate-reactive compound may be a polyol. That is, the coating composition may include the polyurethane resin-forming composition of the above embodiment. The isocyanate-reactive compound may be a polyamine, an amino alcohol, or the like as long as it has two or more isocyanate-reactive groups (eg, active hydrogen groups).

[0128] Since the coating composition includes the polyisocyanate composition of the above embodiment, the coating film has high hardness. The Martens hardness of the coating film at 23° C. is preferably 100 N / mm 2 More preferably 104N / mm 2 More than, more preferably 110N / mm 2 The Martens hardness can be measured in accordance with JIS Z2255.

[0129] The coating film can be formed by applying the coating composition on the surface of the adherend by a known method such as spraying, brushing, dipping, or a coater, and curing the composition.

[0130] The adherend is not particularly limited, and may be an adherend formed using raw materials such as stainless steel, phosphate-treated steel, zinc steel, iron, copper, aluminum, brass, glass, slate, acrylic resin, polycarbonate resin, polyethylene terephthalate resin, polyethylene naphthalate resin, polybutylene terephthalate resin, polystyrene resin, AS resin, ABS resin, polycarbonate-ABS resin, 6-nylon resin, 6,6-nylon resin, MXD6 nylon resin, polyvinyl chloride resin, polyvinyl alcohol resin, polyurethane resin, phenolic resin, melamine resin, polyacetal resin, chlorinated polyolefin resin, polyolefin resin, polyamide resin, polyetheretherketone resin, polyphenylene sulfide resin, NBR resin, chloroprene resin, SBR resin, SEBS resin, or an olefin resin such as polyethylene or polypropylene subjected to corona discharge treatment or other surface treatment, or an adherend having a coating layer that can be formed as an intermediate formed on the surface of the above-mentioned adherend.

[0131] The curing conditions of the coating composition are not particularly limited, but preferably the curing temperature is -5 to 150°C, the humidity is 10 to 95% RH, and the aging time is 0.5 to 336 hours.

[0132] The coating film formed on the surface of the adherend has excellent recoatability and durability, so it is sufficient to form a film thickness of at least 10 microns on the adherend. When the film thickness is 10 microns or more, durability is improved and cracking of the coating film due to impact can be further suppressed.

[0133] Example

[0134] Hereinafter, the contents of the present disclosure will be described in more detail using examples and comparative examples, but the present disclosure is not limited to the following examples.

[0135] <Example 1>

[0136] (Preparation of polyisocyanate composition)

[0137] 800 g of BDI (butane diisocyanate, NCO content: 60.0 mass %) was added to a 1-liter four-necked flask equipped with a stirrer, a thermometer, a cooling tube and a nitrogen inlet tube, heated to 100°C, 9.6 g of hexamethyldisilazane as an isocyanurate catalyst was added, the temperature was raised to 140°C and stirred for 2.6 hours. Then, the temperature was lowered to 50°C with a water bath, 6.0 g of ethanol as a reaction terminator was added, and the reaction was terminated at 50°C for 0.5 hours. After the reaction solution was cooled, the excess BDI was removed by thin film distillation (conditions: 110°C, 0.04 kPa), thereby obtaining 179 g of a polyisocyanate composition P-1 containing a BDI derivative. The properties of the obtained polyisocyanate composition P-1 are shown in Table 1. It should be noted that in this embodiment, the properties of the polyisocyanate composition were determined by the following method.

[0138] (Determination of molar ratio (I / U))

[0139] By using ECX400M (trade name) manufactured by JEOL Ltd. 1 The H-NMR method is used to determine the content of each of the isocyanurate group and the uretdione group (unit: mol %), with the total of the isocyanurate group and the uretdione group in the BDI derivative being 100 mol %, and the molar ratio of the isocyanurate group to the uretdione group (molar ratio (I / U)) is determined from these contents.

[0140] Specifically, first, the polyisocyanate composition was dissolved in deuterated chloroform containing 0.2 mass % of tetramethylsilane to prepare a measurement sample. The sample concentration was 0.02 g / 1 mL mass %. The signal of hydrogen atoms of tetramethylsilane was set to 0 ppm as the chemical shift standard. 1 The measurement sample was measured by H-NMR to determine the signal area of ​​the hydrogen atom of the methylene group adjacent to the nitrogen atom of the isocyanurate ring and the uretdione ring, and the content of the isocyanurate group and the uretdione group was calculated by the following formula.

[0141] Isocyanurate group content (unit: mol%) = (signal area near 3.9 ppm / 6) / (signal area near 3.9 ppm / 6+signal area near 3.3 ppm / 4) × 100

[0142] Uretdione group content (unit: mol%) = (signal area near 3.3 ppm / 4) / (signal area near 3.9 ppm / 6+signal area near 3.3 ppm / 4)×100

[0143] (Determination of content of other BDI derivatives)

[0144] The content and molar ratio (I / U) of compounds derived from BDI monomers other than isocyanurate and uretdione (other BDI derivatives) were calculated in the same manner as described above. 1 The content of other BDI derivatives was determined by the H-NMR method. Specifically, the content of other BDI derivatives was calculated by the following formula.

[0145] Content of other BDI derivatives (unit: mol%) = (signal area near 6.5 to 8.5 ppm + signal area near 4.4 to 5.4 ppm) / (signal area near 3.9 ppm / 6 + signal area near 3.3 ppm / 4 + signal area near 6.5 to 8.5 ppm + signal area near 4.4 to 5.4 ppm) × 100

[0146] (Determination of the content of BDI trimer and BDI dimer)

[0147] The sum of the contents of BDI trimer and BDI dimer (total content) was measured by GPC using the following apparatus.

[0148] Device: HLC-8420 (manufactured by Tosoh Corporation)

[0149] Column: TSKgel (manufactured by Tosoh Corporation)

[0150] G3000H-XL, G2000H-XL, G1000H-XL, 1 each connected in series

[0151] Carrier: Tetrahydrofuran

[0152] Detection method: Differential refractive index detector

[0153] The differential refractive index peak of the aforementioned BDI trimer appears at a retention time of about 23.8 minutes, and the differential refractive index peak of the BDI dimer appears at a retention time of about 24.9 minutes. The areas of these peaks were determined, and the total content of the BDI trimer and BDI dimer was calculated by the following formula.

[0154] Total content of BDI trimer and BDI dimer (mass %) = (peak area at retention time 23.8 minutes + peak area at retention time 24.9 minutes) / total area of ​​all peaks × 100

[0155] (Determination of weight average molecular weight)

[0156] The weight average molecular weight of the obtained polyisocyanate composition (BDI derivative) was measured using the above-mentioned GPC apparatus, with the molecular weight standard being polystyrene.

[0157] (Determination of NCO content)

[0158] The NCO content of the polyisocyanate composition (BDI derivative) is determined by reacting the composition with a secondary amine and then back-titrating the unreacted secondary amine with hydrochloric acid.

[0159] (Viscosity measurement)

[0160] The viscosity of the obtained polyisocyanate composition (BDI derivative) was measured in an environment of 25° C. using a rheometer (HAAKEMARS60, manufactured by Thermo Fisher Scientific Inc.).

[0161] <Example 2>

[0162] 800 g of BDI was added to a 1-liter four-necked flask equipped with a stirrer, a thermometer, a cooling tube and a nitrogen inlet tube, heated to 150°C and stirred for 4 hours. Then 8.0 g of hexamethyldisilazane as an isocyanurate catalyst was added and stirred for 3.6 hours. Then, the temperature was lowered to 50°C in a water bath, 5.0 g of ethanol as a reaction terminator was added, and the reaction was terminated at 50°C for 0.5 hours. After the reaction solution was cooled, excess BDI was removed by thin film distillation (conditions: 110°C, 0.04 kPa), thereby obtaining 227 g of a polyisocyanate composition P-2 containing a BDI derivative. The properties of the obtained polyisocyanate composition P-2 are shown in Table 1.

[0163] <Example 3>

[0164] 800 g of BDI was added to a 1-liter four-necked flask equipped with a stirrer, a thermometer, a cooling tube, and a nitrogen inlet tube, and heated to 100° C. 8.0 g of hexamethyldisilazane as an isocyanurate catalyst was added, and the temperature was raised to 140° C. and stirred for 3.0 hours. Then, the temperature was lowered to 50° C. in a water bath, 5.0 g of ethanol as a reaction terminator was added, and the reaction was terminated at 50° C. for 0.5 hours. After the reaction solution was cooled, the excess BDI was removed by thin film distillation (conditions: 110° C., 0.04 kPa), thereby obtaining 184 g of a polyisocyanate composition P-3 containing a BDI derivative. The properties of the obtained polyisocyanate composition P-3 are shown in Table 1.

[0165] <Example 4>

[0166] 800 g of BDI was added to a 1-liter four-necked flask equipped with a stirrer, a thermometer, a cooling tube and a nitrogen inlet tube, heated to 150°C and stirred for 3 hours. Then, 6.4 g of hexamethyldisilazane as an isocyanurate catalyst was added and stirred for 2.0 hours. Then, the temperature was lowered to 50°C with a water bath, 4.0 g of ethanol as a reaction terminator was added, and the reaction was terminated at 50°C for 0.5 hours. After the reaction solution was cooled, excess BDI was removed by thin film distillation (conditions: 110°C, 0.04 kPa), thereby obtaining 161 g of a polyisocyanate composition P-4 containing a BDI derivative. The properties of the obtained polyisocyanate composition P-4 are shown in Table 1.

[0167] <Example 5>

[0168] 800 g of BDI was added to a 1-liter four-necked flask equipped with a stirrer, a thermometer, a cooling tube, and a nitrogen inlet tube, and heated to 100° C. 3.2 g of hexamethyldisilazane as an isocyanurate catalyst was added, and the temperature was raised to 140° C. and stirred for 4.0 hours. Then, the temperature was lowered to 50° C. in a water bath, 2.0 g of ethanol as a reaction terminator was added, and the reaction was terminated at 50° C. for 0.5 hours. After the reaction solution was cooled, the excess BDI was removed by thin film distillation (conditions: 110° C., 0.04 kPa), thereby obtaining 112 g of a polyisocyanate composition P-5 containing a BDI derivative. The properties of the obtained polyisocyanate composition P-5 are shown in Table 1.

[0169] <Example 6>

[0170] 800 g of BDI was added to a 1-liter four-necked flask equipped with a stirrer, a thermometer, a cooling tube, and a nitrogen inlet tube, and heated to 100° C. 1.6 g of hexamethyldisilazane as an isocyanurate catalyst was added, and the temperature was raised to 140° C. and stirred for 5.0 hours. Then, the temperature was lowered to 50° C. in a water bath, 1.0 g of ethanol as a reaction terminator was added, and the reaction was terminated at 50° C. for 0.5 hours. After the reaction solution was cooled, excess BDI was removed by thin film distillation (conditions: 110° C., 0.04 kPa), thereby obtaining 88 g of a polyisocyanate composition P-6 containing a BDI derivative. The properties of the obtained polyisocyanate composition P-6 are shown in Table 1.

[0171] <Example 7>

[0172] 800 g of BDI was added to a 1-liter four-necked flask equipped with a stirrer, a thermometer, a cooling tube, and a nitrogen inlet tube, and heated to 100° C. 0.8 g of hexamethyldisilazane as an isocyanurate catalyst was added, and the temperature was raised to 140° C. and stirred for 6.0 hours. Then, the temperature was lowered to 50° C. in a water bath, 0.5 g of ethanol as a reaction terminator was added, and the reaction was terminated at 50° C. for 0.5 hours. After the reaction solution was cooled, excess BDI was removed by thin film distillation (conditions: 110° C., 0.04 kPa), thereby obtaining 83 g of a polyisocyanate composition P-7 containing a BDI derivative. The properties of the obtained polyisocyanate composition P-7 are shown in Table 1.

[0173] <Comparative Example 1>

[0174] 800 g of BDI was added to a 1-liter four-necked flask equipped with a stirrer, a thermometer, a cooling tube, and a nitrogen inlet tube, and heated to 90° C. 11.2 g of N-trimethylsilyl-tert-butylamine as an isocyanurate catalyst was added, and stirred for 3.5 hours. Then, the temperature was lowered to 50° C. in a water bath, 3.9 g of ethanol as a reaction terminator was added, and the reaction was terminated at 50° C. for 0.5 hours. After the reaction solution was cooled, excess BDI was removed by thin film distillation (conditions: 110° C., 0.04 kPa), thereby obtaining 84 g of a polyisocyanate composition P-8 containing a BDI derivative. The properties of the obtained polyisocyanate composition P-8 are shown in Table 1.

[0175] <Comparative Example 2>

[0176] 800 g of BDI was added to a 1-liter four-necked flask equipped with a stirrer, a thermometer, a cooling tube and a nitrogen inlet tube, heated to 160°C and stirred for 1 hour. Then 12.0 g of hexamethyldisilazane as an isocyanurate catalyst was added and stirred for 5.6 hours. Then, the temperature was lowered to 50°C with a water bath, 7.5 g of ethanol as a reaction terminator was added, and the reaction was terminated at 50°C for 0.5 hours. After the reaction solution was cooled, excess BDI was removed by thin film distillation (conditions: 110°C, 0.04 kPa), thereby obtaining 339 g of a polyisocyanate composition P-9 containing a BDI derivative. The properties of the obtained polyisocyanate composition P-9 are shown in Table 1.

[0177] <Comparative Example 3>

[0178] 800 g of BDI was put into a 1-liter four-necked flask equipped with a stirrer, a thermometer, a cooling tube and a nitrogen inlet tube, heated to 160°C and stirred for 3 hours. Then the temperature was lowered to 90°C, 7.2 g of N-trimethylsilyl-diethylamine as an isocyanurate catalyst was added, and stirred for 4.3 hours. Then, the temperature was lowered to 50°C with a water bath, 2.5 g of ethanol as a reaction terminator was added, and the reaction was terminated at 50°C for 0.5 hours. After the reaction solution was cooled, the excess BDI was removed by thin film distillation (conditions: 110°C, 0.04 kPa), thereby obtaining 139 g of a polyisocyanate composition P-10 containing a BDI derivative. The properties of the obtained polyisocyanate composition P-10 are shown in Table 1. Since P-10 contains precipitates, the viscosity was not measured. In addition, due to the same reason, the compatibility with the main agent was poor, so the Martens hardness and the curing start temperature were not evaluated.

[0179] <Comparative Example 4>

[0180] 800 g of BDI was added to a 1-liter four-necked flask equipped with a stirrer, a thermometer, a cooling tube and a nitrogen inlet tube, heated to 140°C and stirred for 3 hours. Then, 0.8 g of hexamethyldisilazane as an isocyanurate catalyst was added and stirred for 2.0 hours. Then, the temperature was lowered to 50°C with a water bath, 0.5 g of ethanol as a reaction terminator was added, and the reaction was terminated at 50°C for 0.5 hours. After the reaction solution was cooled, excess BDI was removed by thin film distillation (conditions: 110°C, 0.04 kPa), thereby obtaining 60 g of a polyisocyanate composition P-11 containing a BDI derivative. The properties of the obtained polyisocyanate composition P-11 are shown in Table 1.

[0181] <Comparative Example 5>

[0182] 800 g of HDI (1,6-hexane diisocyanate, NCO content: 49.9% by mass) was added to a 1-liter four-necked flask equipped with a stirrer, a thermometer, a cooling tube and a nitrogen inlet tube, heated to 140°C and stirred for 2 hours. Then, 2.4 g of hexamethyldisilazane as an isocyanurate catalyst was added and stirred for 3.0 hours. Then, the temperature was lowered to 50°C with a water bath, 1.5 g of ethanol as a reaction terminator was added, and the reaction was terminated at 50°C for 0.5 hours. After cooling the reaction solution, the excess HDI was removed by thin film distillation (conditions: 140°C, 0.04 kPa), thereby obtaining 252 g of a polyisocyanate composition P-12 containing an HDI derivative. The properties of the obtained polyisocyanate composition P-12 are shown in Table 1.

[0183] <Comparative Examples 6 and 7>

[0184] Comparative Examples 6 and 7 used C-HXLV (manufactured by Tosoh Corporation) produced from HDI (1,6-hexane diisocyanate) and STABiO D-370 (manufactured by Mitsui Chemicals, Inc.) produced from PDI (1,5-pentane diisocyanate). The properties of each are shown in Table 1.

[0185] <Evaluation>

[0186] (Quick-drying evaluation)

[0187] A coating composition (two-component coating composition) containing the obtained polyisocyanate composition and acrylic polyol was prepared, and the curing start temperature of the coating composition was measured by a rigid pendulum test using RPT-3000W (trade name, manufactured by A&D Co.), thereby evaluating the quick-drying property of the polyisocyanate composition. Specifically, first, acrylic polyol (trade name: ACRYDIC A-801, hydroxyl value: 50 mgKOH / resin g, solid content: 50% by mass, manufactured by DIC Co., Ltd.) and the polyisocyanate composition were blended in a manner such that the hydroxyl group to isocyanate group equivalent ratio was 1:1, and then adjusted with butyl acetate in a manner such that the coating solid content was 50% by mass, thereby obtaining a coating composition. Next, the coating composition was applied to a steel plate (JIS G3141, trade name: SPCC-SB, manufactured by PALTEC Co., Ltd.) in a manner such that the coating film thickness was 20 μm. Next, the steel plate was heated at a heating rate of 2.5° C. / min, and the temperature at which the cycle of the pendulum (frame: FRB-300, edge: RBE-160) began to decay was determined, and this temperature was defined as the curing start temperature of the coating film.

[0188] (Evaluation of coating hardness)

[0189] A coating composition (two-component coating composition) containing the obtained polyisocyanate composition and acrylic polyol was prepared, a coating film (cured film) was formed using the coating composition, and the Martens hardness of the cured film was measured. Specifically, first, acrylic polyol (trade name: Dianal JR5689, hydroxyl value: 67 mgKOH / resin g, solid content: 61% by mass, manufactured by Mitsubishi Chemical Corporation) and a polyisocyanate composition were mixed in a manner such that the hydroxyl group and isocyanate group equivalent ratio became 1:1, and then butyl acetate was used to adjust the coating solid content to 40% by mass, thereby obtaining a coating composition. Next, the coating composition was applied to a steel plate (JIS G3141, trade name: SPCC-SB, treatment method: PF-1077, manufactured by PALTEC) in a manner such that the thickness of the coating film (uncured film) became 20 μm. Then, the coating film was dried for 1 hour under an environment of a temperature of 23° C. and a relative humidity of 50%, and the dried coating film was heat-treated in a dryer at 150° C. for 30 minutes. Next, the heat-treated coating film was aged for 7 days or more at a temperature of 23° C. and a relative humidity of 50% to obtain a coating film (cured film) containing a cured product of the coating composition. The Martens hardness of the obtained coating film (cured film) was measured using HM2000 (trade name, manufactured by Fischer Instruments) in accordance with JIS Z2255.

[0190] [Table 1]

[0191]

[0192] (Evaluation results)

[0193] As shown in Table 1, polyisocyanate compositions P-1 to 7 have low viscosity, and their coatings have good quick-drying properties and coating hardness. In particular, polyisocyanate compositions P-4 to 6 have high levels of viscosity, coating hardness, and quick-drying properties. Polyisocyanate compositions P-8 and 9 have high viscosity and poor workability. Polyisocyanate composition P-10 has poor compatibility with the main agent and is difficult to produce a coating. Polyisocyanate composition P-11 has low viscosity and good quick-drying properties, but the hardness of the coating is insufficient. Polyisocyanate composition P-12 has low viscosity, but both quick-drying properties and coating hardness are poor. Polyisocyanate compositions P-13 and 14 have insufficient quick-drying properties. It can be said that the polyisocyanate compositions of Examples 1 to 7 have low viscosity and excellent workability and quick-drying properties, and the hardness of the resulting coating is excellent.

Claims

1. A butane diisocyanate derivative having an isocyanurate group and a uretdione group, The molar ratio of the isocyanurate group to the uretdione group is 20 / 80 to 80 / 20, The butane diisocyanate derivative has a weight average molecular weight of 790 g / mol or less based on gel permeation chromatography.

2. The butane diisocyanate derivative according to claim 1, comprising butane diisocyanate trimer and butane diisocyanate dimer, The total content of the butane diisocyanate trimer and the butane diisocyanate dimer is 45 to 95% by mass based on the total mass of the butane diisocyanate derivative.

3. The butane diisocyanate derivative according to claim 1, wherein The molar ratio of the isocyanurate group to the uretdione group is 50 / 50 or more.

4. The butane diisocyanate derivative according to claim 1, wherein The molar ratio of the isocyanurate group to the uretdione group is 60 / 40 or less.

5. A method for producing a butane diisocyanate derivative according to any one of claims 1 to 4, comprising: In a first heating step, the reactant containing butane diisocyanate is heated to above 80°C; and In the second heating step, the reactant that has undergone the first heating step is heated at 80 to 180° C. in the presence of an isocyanurate-forming catalyst.

6. The method for producing a butane diisocyanate derivative according to claim 5, wherein: The isocyanuration catalyst includes an aminosilyl group-containing compound. 7 . A polyisocyanate composition comprising the butane diisocyanate derivative according to claim 1 . 8 . The polyisocyanate composition according to claim 7 , which has a viscosity at 25° C. of 2500 mPa·s or less. 9 . A polyurethane resin-forming composition comprising the polyisocyanate composition according to claim 8 and a polyol. 10 . A coating composition comprising the polyisocyanate composition according to claim 8 and a compound having two or more isocyanate-reactive groups. 11 . A coating film comprising a cured product of the coating composition according to claim 10 .

Citation Information

Cited By

  • Polyisocyanate composition, coating composition and application