Method for passivating heavy metals and releasing organic matters in coal gangue or gasified slag

By using calcium oxide and ferric nitrate in coal gangue or gasified slag to generate hydrotalcite, passivate the heavy metal into the crystal lattice and release organic matter, the problems of low removal efficiency of heavy metals and insufficient utilization of organic matter in the prior art are solved. , achieving low-cost and stable heavy metal passivation and organic matter release effects.

CN118950659APending Publication Date: 2024-11-15BEIJING UNIV OF CHEM TECH +1
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202411026820.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The prior art uses a large amount, high energy consumption, high cost, and fails to effectively utilize the organic matter in coal gangue and gasified slag, and fails to fundamentally passivate the heavy metals.

Method used

Use calcium oxide and iron nitrate to mix with coal gangue or gasified slag to generate hydrotalcite, passivate the heavy metal into the hydrotalcite-like lattice, thereby reducing the effective state content of heavy metals, and breaking the coal gangue by generating hydrotalcite-like Or the dissolution balance of the gasified slag releases organic matter.

Benefits of technology

The amount is small, the cost is low, and the passivation effect is stable. It significantly reduces the effective state content of heavy metals and releases rich organic matter and nutrients, which improves the resource utilization rate of coal gangue and gasification slag.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides a method for passivating heavy metals and releasing organic matters in coal gangue or gasified slag. According to the method, a passivating agent reacts with heavy metals in coal gangue and gasified slag to generate hydrotalcite-like compounds, and the heavy metals are passivated in crystal lattices of the hydrotalcite-like compounds, so that the heavy metals are converted into a mineralized state from a free state. Due to the fact that the solubility product constant of the hydrotalcite-like compound is extremely low, passivated heavy metal is difficult to dissociate, and the effective state content of the heavy metal is stably reduced for a long time. Meanwhile, the generated hydrotalcite-like compound breaks the dissolving process of the coal gangue and the gasified slag, and promotes the coal gangue and the gasified slag to release more organic matter nutrients. According to the method, rich organic matter nutrients contained in the coal gangue and the gasified slag can be released while heavy metals in the coal gangue and the gasified slag are passivated, meanwhile, the cost is low, the effect is remarkable, and the method is simple and easy to implement, practical feasibility is provided for resource utilization of the coal gangue and the gasified slag, and wide ecological benefits, economic benefits and social benefits are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of effective utilization of solid waste resources, and in particular to a method for passivating heavy metals and releasing organic matter in coal gangue or gasified slag. Background Art

[0002] Gangue contains a variety of toxic and harmful heavy metal elements, such as lead, cadmium, nickel, chromium and copper. When gangue is exposed to the atmosphere, water and soil environment, these heavy metal elements will be released, polluting the surrounding environment, and will accumulate through the food chain and harm human health. In addition, the heavy metals in gangue make the resource utilization of gangue face a series of challenges. For example, when filling or reclaiming the soil with gangue, it is necessary to consider whether the heavy metals will migrate and pollute the surrounding land and crops. In addition to heavy metals, gangue also contains rich organic matter. Therefore, it is necessary to develop a technology that fully utilizes the organic nutrients contained in gangue and removes heavy metals in gangue, so as to improve the resource utilization rate and ecological value of gangue.

[0003] Similarly, coal gasification slag is a solid waste generated in coal gasification technology, with an annual emission of more than 33 million tons. However, the current disposal methods of coal gasification slag are mainly landfill and stockpiling, and its utilization value is extremely low. Like coal gangue, coal gasification slag is rich in organic matter, but the heavy metals in coal gasification slag also hinder the resource utilization of coal gasification slag.

[0004] Currently, the common method for removing heavy metals from coal gangue or gasification slag is to use microorganisms, mineral materials and eluents to passivate heavy metals.

[0005] Chinese patent CN116903421A discloses a method for passivating heavy metals in coal gangue using microorganisms. The method crushes the coal gangue into powder with a particle size of less than 115 μm, selects SK1 bacteria with fast reproduction speed and high reproduction stability, and mixes the SK1 bacteria with the coal gangue for fermentation. The method uses the metabolites of SK1 bacteria to convert the insoluble phosphorus, potassium and silicon in the coal gangue into effective phosphorus, fast-acting potassium and effective silicon that can be absorbed and utilized by plants, and at the same time uses the three extracellular polymers and cell structure of SK1 bacteria to passivate the lead and chromium in the coal gangue, with passivation rates of 91% and 86% respectively.

[0006] Chinese patent CN114588579 A discloses a method for passivating heavy metals in coal gangue. The method is to use medical stone and zeolite as single passivators, and mix medical stone and zeolite in a mass ratio of 1:1 as a composite passivator to passivate coal gangue. The method can significantly reduce the effective state of heavy metals in coal gangue, and the passivation rate of Cd, Cu, Ni and Pb in coal gangue exceeds 40%, and the heavy metal content in the leaching liquid of coal gangue after passivation is lower than the content requirements of heavy metals in surface water, groundwater and drinking water.

[0007] Chinese patent CN118305172A discloses a method for harmless treatment of heavy metals in coal gangue. In this method, after drying and crushing the coal gangue, it is mixed with one or more passivating agents selected from magnesium oxide, calcium oxide, iron oxide, calcium phosphate, calcite, kaolin and superphosphate in a ratio of 200:1-1:2, maintained at a certain temperature and time, and the effective state of heavy metals in the coal gangue is reduced by oscillation. At the same time, the coal gangue is mixed with one or more eluents selected from formic acid, acetic acid, propionic acid, citric acid, succinic acid and disodium EDTA in a ratio of 200:1-1:200, maintained at a certain speed and time, and filtered to reduce the heavy metal content in the coal gangue.

[0008] Chinese patent CN112430171A discloses a method for preparing an acidic soil conditioner and improving acidified soil using coal gasification slag. The method grinds and screens the gasified slag to 85-90μm, adds calcium oxide, and calcines it at 800-900℃ for 0.8-1.2 hours, then mixes the calcined product with organic matter in a mass ratio of 6:4 to prepare an improver. The improver can turn acidic soil into neutral soil and realize large-scale production of crops. Although the total amount of heavy metals in the improver meets the T / CCEMA 0001-2019 "Soil Water Retention and Conditioning Agent (Fly Ash Based)" standard, it does not pay attention to the changes in the effective heavy metals in the gasified slag.

[0009] The above invention technologies have a certain effect on the removal of heavy metals in coal gangue and gasification slag, but the amount of mineral materials and eluents used is large, the energy consumption is high, and the cost of microbial fermentation is high. Most of the improvement principles are to use the precipitation reaction of heavy metals, without fundamentally passivating heavy metals, and at the same time, they do not pay attention to the release and utilization of organic nutrients in coal gangue and gasification slag.

[0010] In order to solve the above problems, the present invention provides a method for passivating heavy metals in coal gangue or gasified slag and releasing organic matter. The method passivates the heavy metals in coal gangue or gasified slag in the lattice of hydrotalcite (K spThe value is extremely low), so that the heavy metals are changed from the free state to the mineralized state, and the heavy metals are passivated fundamentally, and the effective state content of the heavy metals is reduced. At the same time, the generated hydrotalcite-like heavy metals can break the dissolution balance of coal gangue or gasified slag, so that the organic matter in the coal gangue or gasified slag is released. The passivating agent used in the present invention is small in amount, low in cost, and has a stable passivation effect, which provides a feasible technical approach for the harmlessness and resource utilization of coal gangue or gasified slag. Summary of the invention

[0011] The purpose of the present invention is to provide a method for passivating heavy metals and releasing organic matter in gangue or gasified slag in view of the shortcomings of existing coal gangue or gasified slag heavy metal passivation technology and the lack of research on the release of organic matter in gangue or gasified slag. In this method, calcium oxide and ferric nitrate are mixed with coal gangue or gasified slag respectively, and the heavy metals in the coal gangue or gasified slag can react with calcium ions or iron ions to generate a solubility product constant (K sp ) extremely low hydrotalcite-like substances, which transform heavy metals from free state to mineralized state in the hydrotalcite-like lattice, making it difficult for them to be freed. At the same time, the process of generating hydrotalcite-like substances breaks the dissolution process of coal gangue or gasified slag itself, causing the coal gangue or gasified slag to continuously dissolve and release organic nutrients that can be absorbed and utilized by plants.

[0012] In order to solve the above technical problems, the present invention provides a method for passivating heavy metals and releasing organic matter in coal gangue or gasification slag, comprising the following steps:

[0013] A. Air dry the gangue or gasified slag, grind and crush it, and then pass it through a 2-3 cm sieve.

[0014] B. Apply calcium oxide to the gangue or gasified slag treated in step A and mix them evenly, with the application amount being 0.8-4.8 g per kilogram of gangue or gasified slag; the optimal application amount is 2.24-4.16 g per kilogram of gangue or gasified slag, which serves to provide divalent metal cations for the formation of hydrotalcite-like substances and to disrupt the dissolution process of the gangue or gasified slag.

[0015] C. Add ferric nitrate to the gangue or gasified slag treated in step B and mix them evenly, with the application amount being 2.665-7.995 g per kilogram of gangue or gasified slag; the optimal application amount is 3.731-6.929 g per kilogram of gangue or gasified slag, which serves to provide trivalent metal cations for the formation of hydrotalcite-like substances and disrupt the dissolution process of the gangue or gasified slag.

[0016] D. The amount of water sprayed is 50% of the mass of the gangue or gasified slag, and then water is added to the original moisture content every week according to the dryness of the substrate. The treatment time is at least three months.

[0017] The five-point sampling method is used to sample the passivated gangue or gasification slag every other month. After natural air drying, the contents of effective heavy metals and water-soluble organic carbon in the gangue or gasification slag are determined. The observation is conducted for a total of 3 months.

[0018] The beneficial effects of the present invention are as follows:

[0019] (1) The amount of passivation agent used is small, the cost is low, and the passivation technology is simple and easy.

[0020] (2) Calcium oxide and iron nitrate react with heavy metals in coal gangue or gasification slag to form hydrotalcite-like substances, which in situ passivate the heavy metals in the hydrotalcite-like lattice, and transform the heavy metals from the free state to the mineralized state. Hydrotalcite-like substances have an extremely low solubility product constant, which makes it difficult for heavy metals to be freed, thereby reducing the content of effective heavy metals.

[0021] (3) The hydrotalcite-like substances generated during the passivation process can disrupt the dissolution process of coal gangue or gasified slag, causing the coal gangue or gasified slag to release the rich organic matter contained therein. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Curve diagram of the change of effective content of heavy metals in coal gangue of Example 1 over time

[0023] Figure 2 Curve diagram of the change of effective content of heavy metals in coal gangue of Example 2 over time

[0024] Figure 3 Curve diagram of the change of effective content of heavy metals in coal gangue over time in Example 3

[0025] Figure 4 Curve diagram of the change of water-soluble organic carbon content in coal gangue of Examples 1-3 over time

[0026] Figure 5 Curve diagram of the change of effective content of heavy metals in gasified slag of Example 4 over time

[0027] Figure 6 Curve diagram of the change of water-soluble organic carbon content in the gasified slag of Example 4 over time DETAILED DESCRIPTION

[0028] Example 1

[0029] The present invention is applicable to coal gangue or gasified slag with consistent chemical composition and content. Embodiment 1-4, passivation effect and organic matter release effect Take Wushen Banner Town, Ordos City, Inner Mongolia Autonomous Region as an example, but not limited to this, and coal gangue or gasified slag with consistent chemical composition and content with the local area is applicable.

[0030] The chemical composition and content of the gangue or gasification slag in Wushen Banner Town, Ordos City, Inner Mongolia Autonomous Region are shown in Table 1. The gangue or gasification slag accumulated locally was selected, and the calcium oxide and ferric nitrate were purchased locally. The implementation time was early May, and the specific steps were as follows:

[0031] A. Crush and pulverize large pieces of coal gangue until they can pass through a 2–3 cm sieve.

[0032] B. Add 0.8 g of calcium oxide per kilogram of coal gangue to the coal gangue treated in step A and mix well.

[0033] C. Add 2.665 g of ferric nitrate per kilogram of coal gangue to the coal gangue treated in step B and mix well.

[0034] D. The amount of water sprayed is 50% of the mass of the gangue or gasified slag, and then water is added to the original moisture content every week according to the dryness of the substrate. The five-point sampling method is used to sample the passivated gangue or gasified slag every other month. After natural air drying, the content of effective heavy metals and water-soluble organic carbon in the gangue or gasified slag is determined. The observation is for a total of 3 months ( Figure 1 and Figure 4 ).Depend on Figure 1 and Figure 4 It can be seen that the passivation rate of heavy metals in coal gangue is 61.4%-66.9%, and the release of water-soluble organic carbon is 45.7 mg / kg.

[0035] Table 1 Chemical composition and content of coal gangue and gasified slag

[0036]

[0037]

[0038] Example 2

[0039] A. Crush and pulverize large pieces of coal gangue until they can pass through a 2–3 cm sieve.

[0040] B. Add 3.2 g of calcium oxide per kilogram of coal gangue to the coal gangue treated in step A and mix well.

[0041] C. Add 5.33 g of ferric nitrate per kilogram of coal gangue to the coal gangue treated in step B and mix well.

[0042] D. The amount of water sprayed is 50% of the mass of the gangue or gasified slag, and then water is added to the original moisture content every week according to the dryness of the substrate. The five-point sampling method is used to sample the passivated gangue or gasified slag every other month. After natural air drying, the content of effective heavy metals and water-soluble organic carbon in the gangue or gasified slag is determined. The observation is for a total of 3 months ( Figure 2 and Figure 4 ).Depend on Figure 2 and Figure 4 It can be seen that the passivation rate of heavy metals in coal gangue is 80.4%-86.3%, and the release of water-soluble organic carbon is 98.4 mg / kg.

[0043] Example 3

[0044] A. Crush and pulverize large pieces of coal gangue until they can pass through a 2–3 cm sieve.

[0045] B. Add 4.8 g of calcium oxide per kilogram of coal gangue to the coal gangue treated in step A and mix well.

[0046] C. Add 7.995 g of ferric nitrate per kilogram of coal gangue to the coal gangue treated in step B and mix well.

[0047] D. The amount of water sprayed is 50% of the mass of the gangue or gasified slag, and then water is added to the original moisture content every week according to the dryness of the substrate. The five-point sampling method is used to sample the passivated gangue or gasified slag every other month. After natural air drying, the content of effective heavy metals and water-soluble organic carbon in the gangue or gasified slag is determined. The observation is for a total of 3 months ( Figure 3 and Figure 4 ).Depend on Figure 3 and Figure 4 It can be seen that the passivation rate of heavy metals in coal gangue is 72.0%–76.7%, and the release of water-soluble organic carbon is 62.5 mg / kg.

[0048] Example 4

[0049] A. Grind and sieve the fumed slag until it can pass through a 2-3 cm sieve.

[0050] B. Add 3.2 g of calcium oxide per kg of gasified slag to the gasified slag treated in step A and mix well.

[0051] C. Add 5.33 g of ferric nitrate per kilogram of fumed slag to the fumed slag treated in step B and mix well.

[0052] D. The amount of water sprayed is 50% of the mass of the gangue or gasified slag, and then water is added to the original moisture content every week according to the dryness of the substrate. The five-point sampling method is used to sample the passivated gangue or gasified slag every other month. After natural air drying, the content of effective heavy metals and water-soluble organic carbon in the gangue or gasified slag is determined. The observation is for a total of 3 months ( Figure 5 and Figure 6 ).Depend on Figure 5 and Figure 6 It can be seen that the passivation rate of heavy metals in the gasification slag is 80.8%–85.2%, and the release of water-soluble organic carbon is 55.52 mg / kg.

[0053] Improvement effect verification:

[0054] The present invention samples the local unpassivated coal gangue or gasification slag after 3 months, tests the effective state of heavy metals and the content of water-soluble organic carbon therein, and compares it with the coal gangue or gasification slag after passivation for 3 months in the above 4 embodiments, and the results are shown in Table 2, Table 3, Table 4 and Table 5. Table 2 and Table 3 show that after 3 months, the effective state content of heavy metals in the coal gangue of Example 1, Example 2 and Example 3 all dropped significantly, lower than the coal gangue without passivation treatment, indicating that the heavy metals have been passivated in the hydrotalcite-like lattice. At the same time, the water-soluble organic carbon content is also higher than that of the coal gangue without passivation treatment, indicating that the addition of the passivator can make the coal gangue release more organic nutrients. Table 4 and Table 5 show that after 3 months, the effective state content of heavy metals in the gasification slag of Example 4 is lower than that of the control example, and the water-soluble organic carbon content is greatly increased. The invention has a significant and stable effect of passivating heavy metals in coal gangue or gasified slag, and can release organic nutrients at the same time, greatly tapping the value of coal gangue or gasified slag, and has broad application prospects.

[0055] Table 2 The effective content of heavy metals in coal gangue in different examples at the third month

[0056]

[0057] Table 3 Water-soluble organic carbon content of coal gangue in different examples at the third month

[0058]

[0059] Table 4 Effective content of heavy metals in gasified slag in different embodiments at the third month

[0060]

[0061] Table 5 Water-soluble organic carbon content of gasified slag in different embodiments at the third month

[0062]

Claims

1. A method for passivating heavy metals and releasing organic matter in coal gangue or gasified slag, characterized in that Follow these steps: A. Grind the coal gangue or gasified slag to make it pass through a sieve with a pore size of 2-3 cm; B. adding 0.8-4.8 g of calcium oxide per kilogram of gangue or gasified slag to the gangue or gasified slag treated in step A and mixing evenly; C. applying 2.665-7.995 g of ferric nitrate per kilogram of gangue or gasified slag to the gangue or gasified slag treated in step B, and mixing evenly; D. The amount of water to be sprayed is 50% of the mass of the gangue or gasified slag, and then water is added to the original moisture content every week according to the dryness of the substrate; the treatment time is at least three months.

2. The method for passivating heavy metals and releasing organic matter in coal gangue or gasified slag according to claim 1, characterized in that: The amount of calcium oxide applied in step B is 2.24-4.16 g per kilogram of coal gangue or gasified slag.

3. The method for passivation of heavy metals and release of organic matter in coal gangue or gasified slag according to claim 1, characterized in that: The amount of ferric nitrate applied in step C is 3.731-6.929 g per kilogram of coal gangue or gasified slag.

Citation Information

Patent Citations

  • Method for improving acidified soil by utilizing coal gasification slag and acidified soil conditioner

    CN112430171A

  • Method for passivating metals in coal gangue with abnormal heavy metals by using solid passivator

    CN114588579A

  • Method for passivating heavy metals and activating fertilizer by using microorganisms

    CN116903421A

  • Method for harmlessly treating heavy metals in coal gangue

    CN118305172A

  • Method and apparatus for synthesizing hydrotalcite-like material by using coal gasification furnace residue as aluminum source

    CN105236454A