Tungsten electrode argon arc welding wire and welding part for heat pipe micro-stack welding

By using tungsten argon arc welding wire in heat pipe micro stack, the key element content and welding process are controlled to form a high-temperature and stable austenite structure, the existing welding materials are insufficient in strength and reliability under the environment of 700℃-750℃. The problem has achieved the improvement of the high temperature mechanical properties and corrosion resistance of the weld structure.

CN118951482APending Publication Date: 2024-11-15SHANGHAI NUCLEAR ENGINEERING RESEARCH & DESIGN INSTITUTE CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411077692.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing argon arc welding high-temperature welding materials are difficult to be suitable for use in the service environment of heat pipe micro-stacks at 700℃-750℃, resulting in insufficient strength and reliability of weld structures at high temperatures, making it difficult to meet the requirements of long-term high temperature and high corrosion.

Method used

Using tungsten argon arc welding wire, by controlling the content of elements such as C, Cr, Mo, N, Mn, Zr, etc., a stable austenite structure is formed, which enhances the high-temperature strength and creep resistance of the weld structure, and passes vacuum induction. Furnace smelting and electroslag remelting and smelting reduce impurity content, and combine casting, forging and drawing processes to manufacture welding wires.

Benefits of technology

It improves the mechanical properties, creep properties and corrosion resistance of the weld structure at 700℃-750℃, extends the high-temperature service life of the weld, and significantly improves the welding reliability and safety of heat pipe micro-stack structural parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118951482A_ABST
    Figure CN118951482A_ABST
Patent Text Reader

Abstract

An argon tungsten-arc welding wire for heat pipe micro-heap welding comprises, by weight, 0.04%-0.06% of C, 0.04%-0.06% of N, 0.3%-0.6% of Si, 1.0%-2.0% of Mn, 2.2%-2.7% of Mo, 11.5%-13.5% of Ni, 18.0%-20.0% of Cr, 0.04%-0.1% of Zr and the balance Fe and inevitable impurities, and the impurities comprise less than or equal to 0.015% of P, less than or equal to 0.003% of S, less than or equal to 0.1% of Cu, less than or equal to 0.002% of Sb, less than or equal to 0.001% of Pb, less than or equal to 0.015% of Se, less than or equal to 0.005% of Sn, less than or equal to 0.01% of Zn, less than or equal to 0.005% of O, al < = 0.03%, Ti < = 0.03%, V < = 0.05% and Al + Ti + V < = 0.08%. The argon tungsten-arc welding wire for welding the heat pipe micro-reactor can be used for performing argon tungsten-arc welding on 316H stainless steel, a formed welding seam structure can serve at the temperature of 700-750 DEG C for a long time and keep good strength and corrosion resistance, and the argon tungsten-arc welding wire is suitable for welding reactor cores and reactor bin structural parts of the heat pipe micro-reactor. The invention further provides a welding part.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of nuclear power, and in particular relates to a tungsten inert gas arc welding wire and a welding part for heat pipe micro-stack welding. Background Art

[0002] The heat pipe micro reactor is a solid-state reactor that uses heat pipes for heat transfer. The core structure is simple and compact, with high reliability and good safety, and has good application prospects. At present, the reactor module and stack container of the heat pipe micro reactor are usually welded with 316H stainless steel. During the operation of the heat pipe micro reactor, the structural parts are in a high temperature, high corrosion, and high radiation environment for a long time. They must not only withstand fast neutron irradiation, but also consider the compatibility with the environmental medium (liquid or gaseous sodium). Some key components cannot be replaced during the service period, and the design and manufacturing requirements of the structural parts require a service period of no less than ten years. Therefore, the engineering design puts forward high requirements on the strength, durability and reliability of the 316H stainless steel welded structure. When serving for a long time at a service temperature above 480℃, the failure mechanism of the material changes fundamentally, from ductile failure under short-term high stress conditions to failure dominated by creep under long-term low stress conditions. The maximum service temperature of the existing argon arc welding high-temperature welding materials is 550℃, which is difficult to be applied to the 700℃-750℃ service environment in the heat pipe micro reactor. Therefore, providing a welding material suitable for heat pipe micro-stacks has positive significance for improving the safety and reliability of heat pipe micro-stacks. Summary of the invention

[0003] The purpose of the present invention is to provide a tungsten inert gas arc welding wire for heat pipe micro-stack welding, so as to improve the strength and reliability of the heat pipe micro-stack weld structure at 700° C.-750° C. The present invention also provides a weldment.

[0004] According to an embodiment of one aspect of the present invention, there is provided a tungsten inert gas arc welding wire for heat pipe micro-stack welding, which comprises, by weight, 0.04%-0.06% C, 0.04%-0.06% N, 0.3%-0.6% Si, 1.0%-2.0% Mn, 2.2%-2.7% Mo, 11.5%-13.5% Ni, 18.0%-20.0% Cr, 0.04%-0.1% Zr, and the remainder is Fe and unavoidable impurities. 0.04%-0.06% C, 18.0%-20.0% Cr, 11.5%-14% Ni, 1.0%-2.0% Mn, 0.3%-0.6% Si, 0.05%-0.1% N, 2.2%-2.7% Mo, 0.04%-0.1% Zr, 0.0015%-0.003% B, the balance is Fe and unavoidable impurities, among which, by weight, P≤0.01 5%, S≤0.003%, Cu≤0.1%, Sb≤0.002%, Pb≤0.001%, Se≤0.015%, Sn≤0.005%, Zn≤0.01%, O≤0.005%, H≤0.0005%, Co≤0.06%, Nb≤0.05%, Ca≤0.1%, As≤0.01%, Al≤0.03%, Ti≤0.03%, V≤0.05% and Al+Ti+V≤0.08%.

[0005] C can form carbides with Ni and Cr, thereby enhancing the hardness and wear resistance of stainless steel and ensuring the wear resistance of the material under high-temperature service conditions; at the same time, it can also stabilize austenite at high temperatures, making the weld structure have uniform performance, but C can also form carbides with Cr, resulting in a grain boundary Cr-poor zone, which reduces the intergranular corrosion performance of the material. In the embodiment of the present invention, by controlling the C element, the corrosion performance loss is avoided while maintaining the high-temperature mechanical properties of the material. The Cr element can form carbides, improve the hardness of the structure and the stability of austenite at high temperatures; at the same time, Cr can form a dense oxide film on the surface of stainless steel, inhibiting the oxidation of the structure, and improving the oxidation resistance and corrosion resistance. The Mo element can strengthen the matrix of austenitic stainless steel, improve the high-temperature strength and creep resistance of stainless steel, and enable stainless steel to maintain stable performance during long-term service at high temperatures in heat pipe micro-stacks. The N element is a solid solution strengthening element. While improving the strength of austenitic stainless steel, it does not significantly affect plasticity and toughness. It can also improve the ability of austenitic stainless steel to resist intergranular corrosion, pitting corrosion and crevice corrosion, and can significantly improve the reliability of heat pipe micro-stack structural parts. Mn helps to increase the solubility of N and further improve the strength of the organization. Zr can prevent the austenite structure from coarsening under the high temperature conditions of the heat pipe micro-repile, thereby maintaining the structural stability of the austenite stainless steel microstructure to maintain the mechanical properties and corrosion resistance of the heat pipe micro-repile structural parts under high temperature conditions. Ni is a strong austenite-forming element, which helps to stabilize the structure of austenite under high temperature conditions, improve the high temperature strength of the organization, and inhibit high temperature oxidation. B can improve the thermoplasticity of the material.

[0006] In terms of impurity elements, Al, Ti, and V can strongly promote grain refinement, while refined grains under high temperature conditions will cause serious deterioration of the creep performance of the material. Therefore, in order to maintain the creep resistance of the weld structure under high temperature conditions of 700℃-750℃ that meets the design requirements, it is necessary to limit the content of each element Al, Ti, and V and their total amount to promote the formation of larger grains in the weld after welding. The P element is easy to precipitate and segregate at the grain boundary, significantly reducing the corrosion resistance of chromium-nickel austenitic stainless steel in the solid solution state and sensitized titanium. S and O are easy to form compounds with elements such as Cr and Mn at the grain boundaries, resulting in the depletion of grain boundary alloy elements and reducing intergranular corrosion resistance. Sb, Pb, Se, Sn, Zn, and As will combine with elements such as S and P to form low-melting point compounds and enrich at the grain boundaries. Under high temperature service conditions, it is easy to form liquid cracks, resulting in a significant decline in structural performance. In order to ensure that the weld structure formed by the welding wire has good mechanical properties, creep properties, corrosion resistance and durability under high temperature service conditions of 700℃-750℃,

[0007] Further, in some embodiments, among the unavoidable impurities, by weight, Al≤0.03%, Sb≤0.002%, P≤0.015%, S≤0.003%, Pb≤0.001%, B≤0.0015%, V≤0.05%, Sn≤0.005%, Cu≤0.1%, O≤0.005%, H≤0.0005%, Co≤0.06%, Nb≤0.05%, Ca≤0.1%, As≤0.01%. The service temperature of heat pipe micro-reactor structural parts can reach 700°C, which significantly exceeds the limit temperature of traditional nuclear power facilities, so there are more stringent requirements on the high temperature performance of weld tissue. The presence of impurity elements will have a significant impact on the mechanical properties of the weld tissue at 700°C-750°C, and the content of impurity elements needs to be more strictly controlled.

[0008] Furthermore, in some embodiments, the welding wire is manufactured by vacuum induction furnace smelting and electroslag remelting, and then casting, forging and drawing. Electroslag remelting can effectively reduce the content of impurity elements in the alloy, and achieve more accurate control of the alloy composition, especially the content of sensitive impurities therein.

[0009] Furthermore, in some embodiments, the tungsten inert gas arc welding wire for heat pipe micro-stack further includes pickling and machining steps to remove surface oxide scale before drawing. Removing the oxide scale can further reduce the oxygen content in the welding wire.

[0010] According to an embodiment of another aspect of the present invention, a welded part is provided, comprising a base material and a weld structure, the weld structure comprising a cladding metal formed by melting and solidifying a welding wire, wherein the weld structure comprises a cladding metal formed by melting and solidifying a welding wire, characterized in that the base material is 316H stainless steel, and the composition of the cladding metal comprises, by weight ratio: 0.04%-0.06% C, 18.0%-20.0% Cr, 11.5%-14% Ni, 1.0%-2.0% Mn, 0.3%-0.6% Si, 0.05%-0.1% N, 2.2%-2.7% Mo, 0.04%-0.1% The invention relates to an alloy of nickel and zinc. The alloy comprises: 0.01% Zr, 0.0015%-0.003% B, and the balance is Fe and inevitable impurities, among which, by weight ratio, P≤0.015%, S≤0.003%, Cu≤0.1%, Sb≤0.002%, Pb≤0.001%, Se≤0.015%, Sn≤0.005%, Zn≤0.01%, O≤0.005%, H≤0.0005%, Co≤0.06%, Nb≤0.05%, Ca≤0.1%, As≤0.01%, Al≤0.03%, Ti≤0.03%, V≤0.05% and Al+Ti+V≤0.08%.

[0011] Furthermore, in some embodiments, the volume ratio of delta ferrite in the cladding metal is 3%-8%, the balance is austenite, and the grain size of the cladding metal is level 3-6. Austenite structure has a more stable structure under high-temperature service conditions and better high-temperature mechanical properties; a larger structure grain size makes the cladding metal structure have better creep resistance.

[0012] Furthermore, in some embodiments, the cladding metal has a yield strength of ≥210MPa, a tensile strength of ≥520MPa, an elongation after fracture of ≥30%, and an impact energy of ≥90J at room temperature; a yield strength of ≥110MPa, and a tensile strength of ≥320MPa at 650°C; a yield strength of ≥105MPa, and a tensile strength of ≥265MPa at 700°C; a yield strength of ≥99MPa, and a tensile strength of ≥255MPa at 725°C; and a yield strength of ≥99MPa, and a tensile strength of ≥255MPa at 750°C.

[0013] Furthermore, in some embodiments, after the weld structure is bent 180°, there are no opening defects exceeding 1.5 mm on the tensile surface of the weld structure, and there are no opening defects exceeding 3.0 mm at the fusion line.

[0014] Furthermore, in some embodiments, the weld structure is subjected to an intergranular corrosion test after being sensitized at 675°C for 1 h, and the surface has no cracking tendency and no intergranular corrosion cracks. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 A photo of cladding metal in one embodiment;

[0016] Figure 2 FIG. 4 is a metallographic photograph of the cladding metal in one embodiment.

[0017] The purpose of the above drawings is to explain the present invention in detail so that those skilled in the art can understand the technical concept of the present invention, but it is not intended to limit the present invention. DETAILED DESCRIPTION

[0018] The present invention is further described in detail below through specific embodiments in conjunction with the accompanying drawings.

[0019] Reference to "embodiment" herein means that a particular feature, structure or characteristic described in conjunction with the embodiment may be included in at least one embodiment of the present invention. The phrase appearing in various locations in the specification does not necessarily refer to the same embodiment, nor is it limited to mutually exclusive independent or alternative embodiments. It should be understood by those skilled in the art that the embodiments herein may be combined with other embodiments without structural conflicts. In the description herein, "multiple" means at least two.

[0020] As a new generation of reactor, heat pipe micro reactor does not have a liquid circuit in the reactor. The heat pipe with sodium as the working fluid transmits the fission heat in the reactor to the thermoelectric conversion device. Compared with traditional reactors or fast reactors, the service temperature of heat pipe micro reactor structures is higher. The design requires that they can still be in long-term stable service without failure under high temperature conditions of 750℃; in contrast, the service temperature of existing nuclear power structural materials usually does not exceed 600℃. Usually, the reactor module and stack container of heat pipe micro reactor are welded and manufactured by 316H stainless steel. The existing 316H stainless steel welding materials usually use coated electrodes and welding wire + flux combination. Coated electrodes are suitable for arc welding process, and welding wire + flux combination is suitable for submerged arc welding process. These welding processes are restricted by efficiency and welding conditions, and cannot achieve effective welding of heat pipe micro reactor structures. In addition, the weld structure provided by the existing process is difficult to maintain strength and reliability under high temperature conditions of heat pipe micro reactor service.

[0021] In order to solve the above problems, an embodiment of one aspect of the present invention provides a tungsten inert gas arc welding wire for heat pipe micro-stack welding, which is suitable for 316H stainless steel tungsten inert gas arc welding, can effectively improve the weld quality, is suitable for automated welding, and the formed weld structure can serve stably for a long time under high temperature conditions of 700℃-750℃.

[0022] In one embodiment, the composition of the welding wire includes, by weight ratio, 0.04%-0.06% C, 18.0%-20.0% Cr, 11.5%-14% Ni, 1.0%-2.0% Mn, 0.3%-0.6% Si, 0.05%-0.1% N, 2.2%-2.7% Mo, 0.04%-0.1% Zr, 0.0015%-0.003% B, and the balance is Fe and inevitable impurities. Among the inevitable impurities, by weight ratio In terms of amount ratio, P≤0.015%, S≤0.003%, Cu≤0.1%, Sb≤0.002%, Pb≤0.001%, Se≤0.015%, Sn≤0.005%, Zn≤0.01%, O≤0.005%, H≤0.0005%, Co≤0.06%, Nb≤0.05%, Ca≤0.1%, As≤0.01%, Al≤0.03%, Ti≤0.03%, V≤0.05% and Al+Ti+V≤0.08%.

[0023] C can form carbides with Ni and Cr, thereby enhancing the hardness and wear resistance of stainless steel and ensuring the wear resistance of the material under high-temperature service conditions; at the same time, it can also stabilize austenite at high temperatures, making the weld structure have uniform performance, but C can also form carbides with Cr, resulting in a grain boundary Cr-poor zone, which reduces the intergranular corrosion performance of the material. In the embodiment of the present invention, by controlling the C element, the corrosion performance loss is avoided while maintaining the high-temperature mechanical properties of the material. The Cr element can form carbides, improve the hardness of the structure and the stability of austenite at high temperatures; at the same time, Cr can form a dense oxide film on the surface of stainless steel, inhibiting the oxidation of the structure, and improving the oxidation resistance and corrosion resistance. The Mo element can strengthen the matrix of austenitic stainless steel, improve the high-temperature strength and creep resistance of stainless steel, and enable stainless steel to maintain stable performance during long-term service at high temperatures in heat pipe micro-stacks. The N element is a solid solution strengthening element. While improving the strength of austenitic stainless steel, it does not significantly affect plasticity and toughness. It can also improve the ability of austenitic stainless steel to resist intergranular corrosion, pitting corrosion and crevice corrosion, and can significantly improve the reliability of heat pipe micro-stack structural parts. Mn helps to increase the solubility of N and further improve the strength of the organization. Zr can prevent the austenite structure from coarsening under the high temperature conditions of the heat pipe micro-repile, thereby maintaining the structural stability of the austenite stainless steel microstructure to maintain the mechanical properties and corrosion resistance of the heat pipe micro-repile structural parts under high temperature conditions. Ni is a strong austenite-forming element, which helps to stabilize the structure of austenite under high temperature conditions, improve the high temperature strength of the organization, and inhibit high temperature oxidation. B can improve the thermoplasticity of the material.

[0024] In terms of impurity elements, Al, Ti, and V can strongly promote grain refinement, while refined grains under high temperature conditions will cause serious deterioration of the creep performance of the material. Therefore, in order to maintain the creep resistance of the weld structure under high temperature conditions of 700℃-750℃ that meets the design requirements, it is necessary to limit the content of each element Al, Ti, and V and their total amount to promote the formation of larger grains in the weld after welding. The P element is easy to precipitate and segregate at the grain boundary, significantly reducing the corrosion resistance of chromium-nickel austenitic stainless steel in the solid solution state and sensitized titanium. S and O are easy to form compounds with elements such as Cr and Mn at the grain boundaries, resulting in the depletion of grain boundary alloy elements and reducing intergranular corrosion resistance. Sb, Pb, Se, Sn, Zn, and As will combine with elements such as S and P to form low-melting point compounds and enrich at the grain boundaries. Under high temperature service conditions, it is easy to form liquid cracks, resulting in a significant decline in structural performance. In order to ensure that the weld structure formed by the welding wire has good mechanical properties, creep properties, corrosion resistance and durability under high temperature service conditions of 700℃-750℃,

[0025] The welding wire provided in the above embodiment is melted in a vacuum induction furnace, and then electroslag remelting is performed to further reduce the impurity content and improve the purity, and then the finished welding wire is manufactured through casting, forging and drawing processes. In a preferred embodiment, the welding wire is further pickled and mechanically processed such as washing to remove the oxide scale on the surface before drawing, so as to further reduce the oxygen content in the welding wire.

[0026] The welding wire provided in the above embodiment is used to perform tungsten inert gas arc welding on 316H stainless steel base material to obtain a welded part, and the weld morphology is as follows: Figure 1 As shown in the figure, the weld surface is evenly clad without macroscopic defects, with high welding efficiency and good process stability. The undiluted cladding metal in the weld structure is consistent with the chemical composition of the welding wire. The metallographic structure of the cladding metal is as follows: Figure 2 As shown, the volume ratio of delta ferrite is 3%-8%, and the rest is austenite structure. The weld structure is uniform, without defects such as pores and cracks. When the weld structure of the welded part is in service for a long time under the high temperature conditions of the heat pipe micro-repile, due to the effect of austenitizing elements in the cladding metal, the transformation of the austenite matrix to delta ferrite is inhibited, so that the delta ferrite with lower strength is maintained at a lower volume ratio, so that the overall weld structure maintains higher mechanical properties.

[0027] The weld structure was sampled, and the undiluted cladding metal was sampled to measure the yield strength Rp at room temperature. 0.2 ≥210MPa, tensile strength Rm ≥520MPa, elongation after fracture A ≥30%, impact energy Akv ≥90J. At 650℃, yield strength Rp 0.2 ≥110MPa, tensile strength Rm≥320MPa. At 700℃, yield strength Rp 0.2 ≥105MPa, tensile strength Rm≥265MPa. At 725℃ and 750℃, yield strength Rp 0.2 ≥99MPa, tensile strength Rm≥255MPa. Under 750℃, the elongation after fracture of the cladding metal sample in the tensile test is not less than 20%.

[0028] A transverse bending test is carried out on the weld structure. According to the requirements of AWS B4.0, the specimen containing the weld structure is bent 180°, and the tensile surface of the weld structure of the bent specimen is measured along any direction. There is no open defect exceeding 1.5 mm, and there is no open defect exceeding 3.0 mm at the fusion line of the weld structure.

[0029] The weld structure was subjected to an intergranular corrosion test. According to GB / T 4334E standard, the sample was subjected to a sensitization treatment at 675°C for 1 hour and then subjected to chemical corrosion. In some embodiments, the copper-copper sulfate test method was used. After chemical corrosion, the sample was bent. There was no intergranular corrosion on the tensile surface of the weld structure, and no cracking tendency was found.

[0030] In one embodiment of the present invention, the tungsten inert gas arc welding wire for heat pipe micro-stack welding has the following components by weight percentage: C 0.06%, N 0.06%, Si 0.45%, Mn 1.8%, Al 0.02%, Ti 0.02%, B 0.0003%, Sb 0.001%, P 0.015%, S 0.003%, Mo 2.3%, Ni 12.5%, Cr

[0031] 18.80%, Pb 0.0001%, V 0.005%, Sn 0.003%, Cu 0.05%, O 0.002%, H0.0005%, Co 0.02%, Nb 0.005%, Ca 0.0001%, As 0.005%, Zr 0.05%, Se0.015%, Zn0.01%, and the balance is Fe.

[0032] The welding wire is used to perform tungsten inert gas arc welding on a 316H stainless steel base material to obtain a welded part, which includes the 316H base material and a weld structure, wherein the weld structure includes a non-diluted cladding metal, and its composition is consistent with the original composition of the welding wire.

[0033] Sampling was conducted in the non-diluted cladding metal area, and the results showed that at room temperature, the yield strength was 463MPa, the tensile strength was 550MPa, and the elongation was 36%. The impact energies measured in three impact tests were 278J, 253J, and 269J, respectively. At 650℃, the yield strength was 225MPa, the tensile strength was 350MPa, and the elongation was 23%. At 700℃, the yield strength was 180MPa, the tensile strength was 300MPa, and the elongation was 23%.

[0034] 279MPa, elongation 22%; at 725℃, the yield strength is 160MPa, the tensile strength is 255MPa, and the elongation is 22%; at 750℃, the yield strength is 140MPa, the tensile strength is 256MPa, and the elongation is 21%.

[0035] The microstructure of the cladding metal was analyzed and the volume ratio of delta ferrite (FN) in the three test areas was measured to be 3.3%, 3.5% and 3.9% respectively, and the average grain size was not less than GB / T 6394.

[0036] The size of the grade 6 grains specified in 2017.

[0037] The samples containing the weld structure are subjected to bending tests according to AWS B4.0 standard, so that the weld structure is located in the bending area. After bending 180°, there are no opening defects exceeding 1.5mm when measuring the weld tensile surface in any direction, and there are no opening defects exceeding 3.0mm at the fusion line.

[0038] For the samples containing the weld structure, the intergranular corrosion test was carried out according to GB / T 4334E standard. First, the samples were sensitized at 675℃×1h, then chemically corroded and bent, where the weld structure was located in the bending area. After bending, there were no intergranular corrosion cracks on the tensile surface of the weld structure, and no cracking tendency was shown.

[0039] The welded parts obtained by welding with the welding wire provided in the above embodiments show good strength and corrosion resistance under high temperature conditions of 700℃-750℃, are suitable for welding of heat pipe micro-reactor structural parts, and can effectively improve the welding efficiency and welding reliability of the heat pipe micro-reactor core structure and stack.

[0040] In another embodiment, the tungsten inert gas arc welding wire for heat pipe micro-stack welding has the following components by weight percentage: C 0.05%, N 0.052%, Si 0.45%, Mn 1.7%, Al 0.02%, Ti 0.02%, Sb 0.001%, P 0.013%, S 0.003%, Mo 2.20%, Ni 12.80%, Cr 18.6%, Pb 0.0001%, B 0.0003%, V 0.005%, Sn 0.003%, Cu 0.05%, O 0.0020%, H 0.0005%, Co 0.020%, Nb 0.005%, Ca 0.0001%, As 0.005%, Zr 0.05%, Se 0.015%, Zn 0.01% and the balance is Fe.

[0041] The welding wire is used to perform tungsten inert gas arc welding on a 316H stainless steel base material to obtain a welded part, which includes the 316H base material and a weld structure, wherein the weld structure includes a non-diluted cladding metal, and its composition is consistent with the original composition of the welding wire.

[0042] Sampling was conducted in the non-diluted cladding metal area, and the results showed that at room temperature, the yield strength was 430MPa, the tensile strength was 540MPa, and the elongation was 35%. The impact energies measured in three impact tests were 228J, 200J, and 180J, respectively. At 650℃, the yield strength was 230MPa, the tensile strength was 420MPa, and the elongation was 26%. At 700℃, the yield strength was 160MPa, and the tensile strength was 100MPa.

[0043] 256MPa, elongation 22%; at 725℃, the yield strength is 135MPa, the tensile strength is 260MPa, and the elongation is 21%; at 750℃, the yield strength is 105MPa, the tensile strength is 255MPa, and the elongation is 21%.

[0044] The microstructure of the cladding metal was analyzed and the volume ratio (FN) of delta ferrite in the three test areas was measured to be 3.8%, 3.2% and 4.3% respectively, and the average grain size was not less than GB / T 6394.

[0045] The size of the grade 6 grains specified in 2017.

[0046] The samples containing the weld structure are subjected to bending tests according to AWS B4.0 standard, so that the weld structure is located in the bending area. After bending 180°, there are no opening defects exceeding 1.5mm when measuring the weld tensile surface in any direction, and there are no opening defects exceeding 3.0mm at the fusion line.

[0047] For the samples containing the weld structure, the intergranular corrosion test was carried out according to GB / T 4334E standard. First, the samples were sensitized at 675℃×1h, then chemically corroded and bent, where the weld structure was located in the bending area. After bending, there were no intergranular corrosion cracks on the tensile surface of the weld structure, and no cracking tendency was shown.

[0048] The welded parts obtained by welding with the welding wire provided in the above embodiments show good strength and corrosion resistance under high temperature conditions of 700℃-750℃, are suitable for welding of heat pipe micro-reactor structural parts, and can effectively improve the welding efficiency and welding reliability of the heat pipe micro-reactor core structure and stack.

[0049] In yet another embodiment, the tungsten inert gas arc welding wire for heat pipe micro-stack welding has the following components by weight percentage: C 0.04%, N 0.05%, Si 0.32%, Mn 1.80%, Al 0.02%, Ti 0.02%, Sb 0.002%, P 0.01%, S 0.0015%, Mo 2.3%, Ni 13.5%, Cr 19.00%, Pb 0.0001%, B 0.0005%, V 0.02%, Sn 0.002%, Cu 0.05%, O 0.0005%, H 0.0002%, Co 0.005%, Nb 0.02%, Ca 0.06%, As 0.006%, Zr 0.012%, Se 0.012%, Zn The balance of 0.01% is Fe.

[0050] The welding wire is used to perform tungsten inert gas arc welding on a 316H stainless steel base material to obtain a welded part, which includes the 316H base material and a weld structure, wherein the weld structure includes a non-diluted cladding metal, and its composition is consistent with the original composition of the welding wire.

[0051] Sampling was conducted in the non-diluted cladding metal area, and the results showed that at room temperature, the yield strength was 440MPa, the tensile strength was 530MPa, and the elongation was 34%. The impact energies measured in three impact tests were 206J, 218J, and 226J, respectively. At 650°C, the yield strength was 280MPa, the tensile strength was 410MPa, and the elongation was 25%. At 700°C, the yield strength was 210MPa, the tensile strength was

[0052] 390MPa, elongation 24%; at 725℃, yield strength 130MPa, tensile strength 360MPa, elongation 22%; at 750℃, yield strength 106MPa, tensile strength 355MPa, elongation 21%.

[0053] The microstructure of the cladding metal was analyzed and the volume ratio of delta ferrite (FN) in the three test areas was measured to be 4.2%, 4.8% and 4.9% respectively, and the average grain size was not less than GB / T 6394.

[0054] The size of the grade 6 grains specified in 2017.

[0055] The samples containing the weld structure are subjected to bending tests according to AWS B4.0 standard, so that the weld structure is located in the bending area. After bending 180°, there are no opening defects exceeding 1.5mm when measuring the weld tensile surface in any direction, and there are no opening defects exceeding 3.0mm at the fusion line.

[0056] For the samples containing the weld structure, the intergranular corrosion test was carried out according to GB / T 4334E standard. First, the samples were sensitized at 675℃×1h, then chemically corroded and bent, where the weld structure was located in the bending area. After bending, there were no intergranular corrosion cracks on the tensile surface of the weld structure, and no cracking tendency was shown.

[0057] The welded parts obtained by welding with the welding wire provided in the above embodiments show good strength and corrosion resistance under high temperature conditions of 700℃-750℃, are suitable for welding of heat pipe micro-reactor structural parts, and can effectively improve the welding efficiency and welding reliability of the heat pipe micro-reactor core structure and stack.

[0058] The purpose of the above embodiments is to further explain the present invention in detail in conjunction with the accompanying drawings so that those skilled in the art can understand the technical concept of the present invention. Within the scope of the present invention, the optimization or equivalent replacement of the technical features involved, and the combination of implementation methods in different embodiments without conflict of structure and principle, all fall within the protection scope of the present invention.

Claims

1. A tungsten inert gas arc welding wire for heat pipe micro-stack welding, characterized in that: By weight, including 0.04%-0.06% C, 18.0%-20.0% Cr, 11.5%-14% Ni, 1.0%-2.0% Mn, 0.3%-0.6% Si, 0.05%-0.1% N, 2.2%-2.7% Mo, 0.04%-0.1% Zr, 0.0015%-0.003% B, the balance is Fe and unavoidable impurities, Among the unavoidable impurities, by weight, P≤0.015%, S≤0.003%, Cu≤0.1%, Sb≤0.002%, Pb≤0.001%, Se≤0.015%, Sn≤0.005%, Zn≤0.01%, O≤0.005%, H≤0.0005%, Co≤0.06%, Nb≤0.05%, Ca≤0.1%, As≤0.01%, Al≤0.03%, Ti≤0.03%, V≤0.05% and Al+Ti+V≤0.08%.

2. The argon tungsten arc welding wire for heat pipe micro-stack welding according to claim 1, characterized in that: The tungsten inert gas arc welding wire for heat pipe micro-stack welding is manufactured by smelting in a vacuum induction furnace and electroslag remelting, and then undergoing casting, forging and drawing processes after smelting.

3. The argon tungsten arc welding wire for heat pipe micro-stack welding according to claim 2, characterized in that: The tungsten inert gas arc welding wire for the heat pipe micro-stack further includes pickling and machining steps to remove surface oxide scale before drawing.

4. A welded part, comprising a base material and a weld structure, wherein the weld structure comprises a cladding metal formed by melting and solidifying a welding wire, characterized in that: The parent material is 316H stainless steel, and the composition of the cladding metal, by weight ratio, includes: 0.04%-0.06% C, 18.0%-20.0% Cr, 11.5%-14% Ni, 1.0%-2.0% Mn, 0.3%-0.6% Si, 0.05%-0.1% N, 2.2%-2.7% Mo, 0.04%-0.1% Zr, 0.0015%-0.003% B, the balance is Fe and unavoidable impurities, Among the unavoidable impurities, by weight, P≤0.015%, S≤0.003%, Cu≤0.1%, Sb≤0.002%, Pb≤0.001%, Se≤0.015%, Sn≤0.005%, Zn≤0.01%, O≤0.005%, H≤0.0005%, Co≤0.06%, Nb≤0.05%, Ca≤0.1%, As≤0.01%, Al≤0.03%, Ti≤0.03%, V≤0.05% and Al+Ti+V≤0.08%.

5. The weldment according to claim 4, characterized in that: The volume ratio of delta ferrite in the cladding metal is 3%-8%, the balance is austenite, and the grain size of the cladding metal is level 3-6.

6. The weldment according to claim 4 or 5, characterized in that: The cladding metal Yield strength ≥210MPa, tensile strength ≥520MPa, elongation after fracture ≥30%, impact energy ≥90J at room temperature; Yield strength ≥110MPa at 650℃, tensile strength ≥320MPa; Yield strength ≥105MPa, tensile strength ≥265MPa at 700℃; Yield strength ≥99MPa at 725℃, tensile strength ≥255MPa; The yield strength is ≥99MPa and the tensile strength is ≥255MPa at 750℃.

7. The weldment according to claim 4 or 5, characterized in that: After the weld structure is bent 180°, there are no opening defects exceeding 1.5 mm on the tensile surface of the weld structure, and no opening defects exceeding 3.0 mm at the fusion line.

8. The weldment according to claim 4 or 5, characterized in that: The weld structure was subjected to an intergranular corrosion test after being sensitized at 675°C for 1 hour, and the surface showed no cracking tendency and no intergranular corrosion cracks.