Large-radian optical glass processing technology

Through the process of combining special-shaped glass sheets with graphite molds, combined with CNC processing and polishing processes, the problem of low surface mold traces and contour strength in thermal bending of large-arc optical glass is solved, and the product yield and mechanical strength are improved.

CN118954919AActive Publication Date: 2024-11-15BIEL OPTIC HUIZHOU +2
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411339073.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-15
Estimated Expiration
2044-09-25

AI Technical Summary

Technical Problem

During the thermal bending process, large-arc optical glass is prone to surface mold marks, low edge strength in the area of ​​sudden contour change, and high product defect rate.

Method used

The combination of special-shaped glass sheets and graphite molds is adopted to form special-shaped glass sheets by cutting the original glass sheets and matching the insert components for limiting. The preheating, forming, slow cooling and fast cooling processes of graphite molds are used to combine CNC processing and polishing processes. , remove the indentation and concave points on the surface of the glass sheet after hot bending, improve the contour strength and improve the product yield.

Benefits of technology

It effectively improves the mold indentation problem of the glass sheet surface, improves the sudden change of contour area and edge strength, improves the yield of thermal bending, and ensures the mechanical strength and appearance quality of the glass sheet.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954919A_ABST
    Figure CN118954919A_ABST
Patent Text Reader

Abstract

The large-radian optical glass processing technology comprises the following steps: cutting a raw glass sheet to obtain a special-shaped glass sheet; a graphite mold is prepared and comprises a lower mold with the upper surface provided with a curved-surface groove, an upper mold with the lower surface forming an arc surface and an insert assembly, the curved-surface groove is provided with a first forming area and a second forming area, and the upper surface of the lower mold is provided with a first clamping groove, a second clamping groove, a third clamping groove and a fourth clamping groove; the height limiting block is correspondingly embedded into the first clamping groove and the second clamping groove and attached to the edge of the special-shaped glass sheet, the first check block and the second check block are correspondingly embedded into the third clamping groove and the fourth clamping groove and attached to the edge of the special-shaped glass sheet, and the height limiting block, the first check block and the second check block are provided with cambered surface structures abutting against the rabbet body of the special-shaped glass sheet. The mold closing gap height of the graphite mold is the thickness of the target large-radian optical glass; putting the special-shaped glass sheet into the curved groove of the lower mold, closing the mold, and preheating, molding, slowly cooling and quickly cooling the graphite mold; carrying out CNC (Computer Numerical Control) processing and finishing on the hot-bent glass sheet; comprehensively polishing the glass sheet; and carrying out chemical hardening and re-polishing on the glass sheet.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of curved glass processing, and in particular to a large-curvature optical glass processing technology. Background Art

[0002] VR head-mounted display (VR head-mounted display device) is a product that combines simulation technology with computer graphics, human-computer interface technology, multimedia technology, sensor technology, network technology and other technologies. It is a new means of human-computer interaction created with the help of computers and the latest sensor technology. VR lenses are an important part of VR head-mounted display. At present, the industry mainly uses large-curved optical glass to make VR lenses to meet the requirements of VR head-mounted display for volume, FOV (Field of View, the range that the lens can cover), imaging quality and cost. Among the different processing technologies of large-curved optical glass, the large-curved optical glass processed by hot bending has the advantages of high appearance, lightness, transparency, cleanliness, anti-fingerprint, anti-glare, hardness, scratch resistance, and good weather resistance. It can bring great improvements in texture, feel, appearance and many other aspects, and thus become the mainstream method of large-curved optical glass processing. The glass hot bending forming process is a method of pressing the 2D glass in a high viscoelastic state in the mold into a large-curvature optical glass by closing the prefabricated mold up and down. During the mold closing process, the mold presses the viscoelastic glass into a shape identical to the mold core surface to make a large-curvature optical glass that meets the design requirements. Compared with the material removal processing method, the hot bending forming method does not require other forming mechanical processing, and the product productivity is significantly improved.

[0003] The factors that affect the quality of hot bending of large-curve optical glass mainly include the following: 1) the heating efficiency of the hot bending machine, the uniformity of the temperature field of the heating structure, the hot bending speed control, and the cooling rate control; 2) the influence of the mold material. The mold must have the characteristics of easy processing, high hardness, high temperature resistance, small thermal expansion coefficient, and long service life. At present, the materials used to make glass molds are mainly graphite, cemented carbide WC, SiC and other materials; 3) the influence of heating temperature. The temperature of the glass is difficult to measure during heating. The technical personnel can only adjust the process parameters based on their experience. The adjustment range is large, and it is difficult to accurately confirm whether the temperature field of the heated glass in the mold is uniform and suitable for hot bending, and it is difficult to determine the shortest heating time. At present, the hot bending process of large-curvature optical glass is mainly divided into a preheating stage, a molding stage, a slow cooling stage and a fast cooling stage. In the preheating stage, the flat glass is placed in a corresponding graphite mold and heated to the softening point of the glass; in the molding stage, the glass that has reached the softening point maintains the molding temperature while applying pressure to the mold according to preset parameters, so that the softened glass replicates the shape of the mold cavity; in the slow cooling stage, the glass is slowly cooled at the annealing temperature to eliminate the thermal stress caused by the expansion of the glass due to temperature increase; in the fast cooling stage, a cooling plate with cooling water passed through it is used to quickly cool the annealed large-curvature optical glass to obtain the product.

[0004] When the above-mentioned hot bending process is used, during the hot bending process of large-curved optical glass, due to product design reasons, the local pressure and temperature are not exactly the same as their corresponding design values, and mold marks on the product surface are difficult to avoid. Secondly, the product contour will change during chemical strengthening of the glass, which will affect the product consistency and yield rate. In addition, due to product structural design reasons, the strength of the product contour sudden change area and edge is relatively low, which makes the product easy to break, further increasing the product defect rate. Summary of the invention

[0005] Based on this, it is necessary to provide a large-curvature optical glass processing technology that can improve the mold indentation on the product surface, enhance the strength of the product contour sudden change area and edge, and improve the product hot bending yield rate in response to the above-mentioned shortcomings.

[0006] A large-curvature optical glass processing process comprises the following steps:

[0007] S1. Cutting the original glass sheet to obtain a special-shaped glass sheet, wherein the special-shaped glass sheet has a runway-shaped structure, wherein two arcuate short side surfaces of the special-shaped glass sheet respectively form a first body-holding limit area, an arcuate long side surface of one side of the special-shaped glass sheet forms a second body-holding limit area, and the middle portion of the arcuate long side surface of the other side of the special-shaped glass sheet is concave to form a nose bridge limit area, and the special-shaped glass sheet is provided with a non-transition area in the middle thereof and a transition area surrounding the non-transition area;

[0008] S2. Prepare a graphite mold, which includes a lower mold, an upper mold covered on the lower mold by plugging, and an insert assembly detachably mounted on the lower mold, wherein the lower portion of the upper mold is formed with an arc surface that abuts against the upper surface of the special-shaped glass piece, and the shape of the arc surface is adapted to the concave shape of the target large-curvature optical glass; a curved groove for accommodating the special-shaped glass piece is provided in the middle portion of the upper surface of the lower mold, and the inner surface shape of the curved groove is adapted to the convex shape of the target large-curvature optical glass, and the inner surface of the curved groove has a first molding area corresponding to the transition area and a second molding area corresponding to the non-transition area and located below the first molding area; the lower mold has a first direction along the length direction of the lower mold and a second direction along the width direction of the lower mold, and the lower mold The upper surface is provided with a first card slot and a second card slot opened at two opposite sides of the curved groove along the first direction, and a third card slot and a fourth card slot opened at two opposite sides of the curved groove along the second direction. The insert assembly includes two height limiting blocks which are respectively embedded in the first card slot and the second card slot and respectively fit with the two first body-standing limiting areas, a first stopper which is embedded in the third card slot and fits with the second body-standing limiting area, and a second stopper which is embedded in the fourth card slot and fits with the nose bridge limiting area; the height limiting block, the first stopper and the second stopper are respectively provided with an arc surface structure for limiting the position of the special-shaped glass piece and abutting against the body of the special-shaped glass piece, the shape of the arc surface structure is adapted to the body shape of the special-shaped glass piece, and the mold clearance height between the upper mold and the lower mold is the thickness of the target large-arc optical glass;

[0009] S3, placing the shaped glass piece into the curved groove of the lower mold, and closing the upper mold cover on the upper part of the shaped glass piece, sending the closed graphite mold to the hot bending machine, and performing preheating, molding, slow cooling and fast cooling in sequence; the preheating temperature of the graphite mold is between 690°C and 810°C, the molding temperature of the graphite mold is between 670°C and 795°C, the slow cooling temperature of the graphite mold is between 380°C and 680°C, and the fast cooling temperature of the graphite mold is 25°C;

[0010] S4, taking out the hot-bent glass sheet, and performing CNC processing and trimming on the shape of the glass sheet;

[0011] S5, taking out the glass piece after CNC processing and polishing the glass piece comprehensively;

[0012] S6. Chemically harden and re-polish the polished glass sheet in sequence to obtain the target large-curvature optical glass.

[0013] In one embodiment, the second molding area is a concave arc structure, the first molding area is a smooth curved surface, and the angle between the first molding area and the first direction or the angle between the first molding area and the second direction is 35°-55°.

[0014] In one embodiment, the first stopper and the second stopper are respectively in a T-shaped structure, two first ear grooves connected to the third slot are provided on both sides of the slot opening of the third slot, and two second ear grooves connected to the fourth slot are provided on both sides of the slot opening of the fourth slot.

[0015] In one of the embodiments, a first arc-shaped groove is provided on a side surface of the height limiting block adjacent to the curved groove; a middle portion of a side surface of the first stopper adjacent to the second body limiting area is raised to form a first raised portion, and a second arc-shaped groove is provided on a side surface of the first raised portion adjacent to the curved groove; a middle portion of a side surface of the second stopper adjacent to the nose bridge limiting area is raised to form a second raised portion, a clamping area is formed between the second raised portion and the nose bridge limiting area, a limiting groove connected to the fourth slot is provided on the upper surface of the lower mold at the clamping area, a nose bridge supporting block respectively supported by the second raised portion and the nose bridge limiting area is inserted in the limiting groove, the depth of the limiting groove is less than the height of the nose bridge supporting block, and the shape of the side of the nose bridge supporting block adjacent to the nose bridge limiting area is adapted to the shape of the nose bridge limiting area.

[0016] In one embodiment, a plurality of guide pillars protruding from the lower surface of the upper mold are spaced apart on the inner side of the lower portion of the upper mold, and a plurality of rails for slidingly fitting the guide pillars in a one-to-one correspondence are provided on the upper surface of the lower mold.

[0017] In one of the embodiments, the upper surface of the upper mold is provided with a hollow structure and a plurality of protrusions, and the weight of the upper mold is 1.33-1.46 kg.

[0018] In one embodiment, step S5 comprises:

[0019] S51, polishing the CNC machined trimming area using a polishing rod;

[0020] S52. Polish the concave and convex surfaces of the glass treated with the polishing rod using a polishing machine and a sponge head.

[0021] In one embodiment, step S51 includes:

[0022] The edge of the glass is polished by using a polishing rod with a polyurethane polishing pad on the surface and nano-cerium oxide polishing liquid.

[0023] The large-curved optical glass processing technology of the present invention is implemented to polish, chemically strengthen and re-polish the glass sheet after heat bending treatment, and while ensuring the mechanical strength of the glass sheet, the indentation or concave-convex point defects caused by heat bending on the surface of the glass sheet can be removed, thereby improving the mold indentation problem on the product surface; when the glass sheet is fully polished, the scars in the area where the contour of the glass sheet suddenly changes, the chamfers and the body parts are eliminated, and the strength of the area where the contour of the glass sheet suddenly changes and the edge parts is improved; the special-shaped glass sheet is limited by the insert assembly, which can effectively avoid the relative movement of the glass horizontally and upwardly, so that The obtained special-shaped glass piece can only be deformed downward and replicate the shape of the mold cavity when softened due to the weight of the upper mold and the pressure of the external cylinder. Since the mold gap between the upper mold and the lower mold is the thickness of the target large-arc optical glass, the weight of the glass is controlled while ensuring the strength of the glass. In addition, the gravity of the glass and the friction between the glass and the graphite mold can prevent the glass piece from shifting during the hot bending process. The slow cooling temperature of the graphite mold is between 380℃-680℃ to avoid wrinkles caused by pulling the material during glass molding, uneven glass thickness and other defects, thereby improving the hot bending yield of the product. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 A schematic diagram of the structure of a special-shaped glass sheet in one embodiment of the present invention;

[0025] Figure 2 It is a schematic diagram of the structure of a graphite mold after mold closing and before hot bending in one embodiment of the present invention;

[0026] Figure 3 It is a schematic diagram of the structure of the hot bending of the graphite mold after mold closing in one embodiment of the present invention;

[0027] Figure 4 for Figure 3 A schematic diagram of the cross-sectional structure of the graphite mold in the illustrated embodiment;

[0028] Figure 5 It is a schematic diagram of the explosion structure of a graphite mold in one embodiment of the present invention;

[0029] Figure 6 A schematic diagram of the structure of an upper mold in one embodiment of the present invention;

[0030] Figure 7 A schematic diagram of the structure of a lower mold in one embodiment of the present invention;

[0031] Figure 8 A bottom view of a graphite mold in one embodiment of the present invention;

[0032] Fig. 9 It is a structural schematic diagram of a height limiting block in one embodiment of the present invention;

[0033] Fig.10 A schematic diagram of the structure of a first stopper and a second stopper in one embodiment of the present invention;

[0034] Fig.11 It is a schematic diagram of the structure of a nose bridge supporting block in one embodiment of the present invention. DETAILED DESCRIPTION

[0035] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.

[0036] The present invention discloses a large-radius optical glass processing technology that can compensate for the change in hardened contour of a product, improve mold indentations on the product surface, enhance the aesthetics and special effects of the product, and enhance the sudden change area and edge strength of the 3D curved glass contour of the product. The processing technology optimizes the structure of a glass sheet to be formed and the structure of a graphite mold for hot-bending the glass sheet, and simultaneously performs CNC, concave-convex surface polishing, hardening and back-polishing on the hot-bent glass sheet, thereby improving the surface quality of the curved glass product.

[0037] For details, please combine Figure 1-11 The large-curvature optical glass processing process of this embodiment includes the following steps:

[0038] S1. Cutting the original glass sheet to obtain the shaped glass sheet 10. In this embodiment, the large-curvature optical glass 20 to be processed and formed is a 3D optical glass for a VR head display. The shaped glass sheet 10 is cut from a rectangular glass sheet. The shaped glass sheet 10 is in a runway-shaped structure (can also be regarded as an approximately elliptical structure), which includes an arc-shaped long side and an arc-shaped short side. The two arc-shaped short side sides of the shaped glass sheet 10 (the convex part of the short side of the shaped glass sheet 10) respectively form a first standing position limiting area 101, and the arc-shaped long side side of one side of the shaped glass sheet 10 (the convex part of the long side of the shaped glass sheet 10) forms a second standing position limiting area 102. The middle part of the arc-shaped long side side of the other side of the shaped glass sheet 10 is concave to form a nose bridge limiting area 103. The shaped glass sheet 10 is provided with a non-transition area located in the middle thereof and a transition area surrounding the non-transition area. It can be understood that, in this embodiment, the shaped glass sheet 10 is a planar structure, and its appearance is similar to the common eye mask structure on the market; the first body limit area 101, the second body limit area 102 and the bridge of the nose limit area 103 are the body of different parts of the shaped glass sheet 10 (i.e., the side surface of the ring in the thickness direction of the glass sheet), and when the shaped glass sheet 10 is hot-bent and worn, the first body limit area 101 corresponds to the cheeks of the user, the second body limit area 102 corresponds to the forehead of the user, and the bridge of the nose limit area 103 corresponds to the bridge of the nose of the user. Further, the thickness of the shaped glass sheet 10 is 0.8±0.01mm, the length of the shaped glass sheet 10 is 198.38±0.01mm, the width of the shaped glass sheet 10 is 99.27±0.01mm, and the width of the narrowest part of the shaped glass sheet 10 corresponding to the bridge of the nose limit area 103 is 82.45±0.01mm.

[0039] It should be noted that the large-arc optical glass 20 of this embodiment refers to a structure with a 3D arc surface and an overall mask-like shape formed after the special-shaped glass sheet 10 is hot-bent. This structure is used to carry electronic products after assembly to realize the functions of displaying images, optical adjustment, protecting user eyes, and providing immersive experience of VR headsets.

[0040] S2. Prepare the graphite mold 30. The graphite mold 30 includes a lower mold 310, an upper mold 320 covering the lower mold 310 by plugging, and an insert assembly detachably mounted on the lower mold 310. In this embodiment, the upper mold 320 and the lower mold 310 are detachably connected via guide pillars. Specifically, a plurality of guide pillars 321 protruding from the lower surface of the upper mold 320 are arranged at intervals on the inner side of the lower portion of the upper mold 320, and a plurality of rails are provided on the upper surface of the lower mold 310 for slidingly mounting the guide pillars 321 in a one-to-one correspondence. Furthermore, the corners of the ring side surface of the lower mold 310 are recessed to form a plurality of arc surfaces that are spaced apart and extend along the height direction of the lower mold 310 and penetrate the upper surface of the lower mold 310. The arc surface has an arc surface 311 and two planes 312 located on both sides of the arc surface and connected to the arc surface. The arc surface 311 and the planes 312 on both sides thereof together constitute a rail. Through the sliding cooperation between the rail and the guide column 321, while achieving the limiting between the upper mold 320 and the lower mold 310, the guiding of the upper mold 320 and the lower mold 310 during assembly can be achieved to reduce the difficulty of closing the upper mold 320 and the lower mold 310. In one embodiment, the guide post 321 is designed with an outward-expanding draft angle, and the entire rail including the arc surface 311 and the plane 312 is provided with an inward-retracting draft angle adapted to the outward-expanding draft angle of the guide post 321. In this way, during the assembly process of the graphite mold 30, after the upper mold 320 and the lower mold 310 are molded together, the upper mold 320 is lowered along the rail through the guide post 321 under the action of its own weight until the arc surface of the upper mold 320 abuts against the upper surface of the glass sheet, and the load-bearing capacity of the glass sheet is the weight of the entire upper mold 320. Further preferably, the side of the guide post 321 is provided with a first outward-expanding draft angle of 10-20°, and the entire rail including the arc surface 311 and the plane 312 is provided with a second inward-retracting draft angle of 10-20°, so as to reduce the difficulty of mold closing and mold opening of the graphite mold 30. The upper mold 320 is opened and closed by means of guide pins 321 and rails. This design can effectively avoid lateral and longitudinal relative movement between the upper mold 320 and the lower mold 310 during the hot bending of the glass sheet, ensuring that the softened glass can smoothly replicate the shape of the clamping space through the weight of the upper mold 320 and the pressure applied to the upper mold 320 by the cylinder of the pressure system.

[0041] The lower part of the upper mold 320 is formed with a curved surface 322 that abuts against the upper surface of the special-shaped glass piece 10. The shape of the curved surface 322 is adapted to the concave shape of the target large-radius optical glass 20. The middle part of the upper surface of the lower mold 310 is provided with a curved surface groove 313 for accommodating the special-shaped glass piece 10. The inner surface shape of the curved surface groove 313 is adapted to the convex shape of the target large-radius optical glass 20. In this way, when the upper mold 320 and the lower mold 310 are molded and no longer slide relative to each other, a mold space is formed between the curved surface 322 and the curved surface groove 313. In this way, the softened special-shaped glass piece 10 is shaped by the co-extrusion of the curved surface 322 and the inner surface of the curved surface groove 313, so that the special-shaped glass piece 10 is softened and fits the inner surface of the curved surface 322 and the curved surface groove 313, so that the special-shaped glass piece 10 replicates the shape of the mold space, so as to obtain a large-radius optical glass 20 blank.

[0042] The inner surface of the curved groove 313 has a first molding area corresponding to the transition area and a second molding area 3132 corresponding to the non-transition area and located below the first molding area 3131. The lower mold 310 has a first direction along the length direction of the lower mold 310 and a second direction along the width direction of the lower mold 310. Further, the second molding area 3132 is a concave arc structure, the first molding area 3131 is a smooth curved surface, and the angle between the first molding area 3131 and the first direction or the angle α between the first molding area 3131 and the second direction is 35°-55°. It can also be understood that the angle between the first molding area 3131 and the lower surface of the lower mold 310 is 35°-55°, that is, the first molding area 3131 has a certain slope. The first molding area 3131 is designed to be a smooth curved surface structure, which ensures that after the preheating of the shaped glass piece 10 is completed, when the temperature of the shaped glass piece 10 reaches the softening point Tf, the shaped glass piece 10 is deformed under the action of the deadweight of the upper mold 320 and does not undergo a sudden change when passing through the first molding area 3131, so that the hot bending of the large-curved optical glass 20 to achieve the final curved surface structure can be smoothly implemented, that is, the slope structure can avoid the generation of a sudden change when the shaped glass piece 10 is formed into a large-curved optical glass 20.

[0043] The upper surface of the lower mold 310 is provided with a first card slot 314 and a second card slot 315 opened on two opposite sides of the curved groove 313 along the first direction, and a third card slot 316 and a fourth card slot 317 opened on two opposite sides of the curved groove 313 along the second direction. It can also be understood that the first card slot 314 and the second card slot 315 are located on the left and right sides of the curved groove 313, and the third card slot 316 and the fourth card slot 317 are located on the front and back sides of the curved groove 313.

[0044] The insert assembly includes two height limiting blocks 330 which are respectively embedded in the first and second slots 314 and 315 and respectively fit with the two first body-standing limiting areas 101, a first stopper 340 which is embedded in the third slot 316 and fit with the second body-standing limiting area 102, and a second stopper 350 which is embedded in the fourth slot 317 and fit with the bridge of nose limiting area 103. The height limiting blocks 330 not only limit the two arc-shaped short sides of the special-shaped glass sheet 10, but also limit the depth of the arc surface 322 of the upper mold 320 embedded in the curved surface groove 313 of the lower mold 310, so as to control the height of the mold space. The height limiting blocks 330, the first stopper 340 and the second stopper 350 are respectively provided with arc surface structures which are used to limit the special-shaped glass sheet 10 and abut against the body of the special-shaped glass sheet 10, and the shape of the arc surface structures is adapted to the body shape of the special-shaped glass sheet 10. By providing a curved surface structure on the height limiting block 330, the first stopper 340 and the second stopper 350, the accurate positioning of the flat glass (shaped glass sheet 10) to be hot-bent can be ensured, and the mold mark generated when the flat glass is hot-bent can be reduced.

[0045] Furthermore, the first stopper 340 and the second stopper 350 are respectively in a T-shaped structure, and two first ear grooves 3161 communicating with the third slot 316 are provided on both sides of the slot of the third slot 316, and two second ear grooves 3171 communicating with the fourth slot 317 are provided on both sides of the slot of the fourth slot 317, so that the insertion depth of the first stopper 340 and the second stopper 350 is limited while limiting the position of the first stopper 340 and the second stopper 350. In addition, the upper surface of the lower mold 310 is respectively provided with two first slots 314 and two second slots 315 on two opposite sides of the curved groove 313, and correspondingly, two blocks 331 are arranged at intervals at the bottom of the height limiting block 330, which are inserted into the two first slots 314 or the two second slots 315 in a one-to-one correspondence, so as to prevent the height limiting block 330 from rotating on the upper surface of the lower mold 310. In this embodiment, a first arc-shaped groove 332 is provided on a side of the height limit block 330 adjacent to the curved groove 313; a middle portion of a side of the first stopper 340 adjacent to the second body limiting area 102 is raised to form a first raised portion 341, and a second arc-shaped groove 342 is provided on a side of the first raised portion 341 adjacent to the curved groove 313; a middle portion of a side of the second stopper 350 adjacent to the nose bridge limiting area 103 is raised to form a second raised portion 351, and a clamping area is formed between the second raised portion 351 and the nose bridge limiting area 103, and the upper portion of the lower mold 310 is A limiting groove 318 connected to the fourth slot 317 is provided on the surface at the clamping area, and a nose bridge supporting block 360 is inserted in the limiting groove 318 to respectively abut against the second protrusion 351 and the nose bridge limiting area 103. The depth of the limiting groove 318 is less than the height of the nose bridge supporting block 360, and the shape of the side of the nose bridge supporting block 360 adjacent to the nose bridge limiting area 103 is adapted to the shape of the nose bridge limiting area 103, so that the insert assembly can be completely fitted with the body of the special-shaped glass piece 10 to avoid mold indentations on the edge and body of the glass after hot bending.

[0046] Furthermore, the height of the assembled height limiting block 330 above the upper surface of the lower mold 310 is the limit height of the graphite mold 30. The upper surface of the height limiting block 330 is provided with a step 333 adjacent to the first arc-shaped groove 332. Different gradients are designed for the height of the step 333 to match molds with different wear heights. In other words, by designing multiple height limiting blocks with different step 333 heights, molds with different wear heights can be met. In this way, the needs of hot-bent glass of different thicknesses can be matched and the number of molds opened can be reduced. When the height limiting block 330 is worn, the mold can be prevented from being scrapped. This can save mold processing time and avoid unnecessary waste in the mold development stage. In addition, R angles are set at the edges of the upper mold 320 and the lower mold 310. This can prevent stress cracking of the mold and cracking of the product due to stress concentration, reduce the difficulty of inserting the product into the mold, avoid interference between the special-shaped glass piece 10 and the upper mold 320 and the lower mold 310, and avoid defects such as collapse and cracking of the mold due to bumps or improper operation during processing, transportation and operation.

[0047] It should be noted that, in this embodiment, the mold clearance height between the upper mold 320 and the lower mold 310 is the thickness of the target large-curved optical glass 20, because the contour design of the large-curved optical glass 20 remains unchanged, that is, the area of ​​the large-curved optical glass 20 remains unchanged, and a reasonable thickness design can not only ensure the strength of the glass, but also achieve control of the weight of the glass. In addition, the gravity of the glass and the friction between the glass and the graphite mold can prevent the glass sheet from being offset during the hot bending process, so as to avoid wrinkles caused by pulling the material during the molding of the large-curved optical glass 20, uneven glass thickness and other defects, and reduce the product defect rate. In addition, the upper surface of the upper mold 320 is provided with a hollow structure and a plurality of protrusions 323. The design height of the protrusions 323 is 0.2 mm. The hollow structure includes a recessed area located in the middle of the upper surface of the upper mold 320 and two temperature measuring holes located on both sides of the recessed area. The depth of the temperature measuring hole is 5 mm and the diameter of the temperature measuring hole is 12 mm. By arranging the protrusions 323 on the upper surface of the upper mold, the tungsten steel plate acting on the cylinder of the graphite mold during hot bending can be prevented from fitting the graphite mold, thereby lifting the graphite mold; similarly, the lower surface of the lower mold is also provided with a protrusion structure 319, which is used to reduce the friction area between the lower mold and the heating plate (i.e., the tungsten steel plate), reduce the dust generated by graphite shedding, and at the same time reduce the force of the lever acting on the mold when the mold is transported in the hot bending machine, thereby reducing the probability of damage to the graphite mold and the lever; the weight of the upper mold 320 is 1.33-1.46 kg. In this embodiment, the upper mold 320 includes an annular baffle, an annular support portion connected to the upper edge of the annular baffle, a bowl-shaped crimping portion located inside the annular baffle and fixedly connected to the inner edge of the annular support portion, the bowl-shaped crimping portion forms a recessed area on the upper surface of the upper mold, the lower surface of the bowl-shaped crimping portion forms an arc surface 322, the guide column 321 is fixed to the inner wall surface of the annular baffle, and the thickness of the thinnest position of the hollow structure part on the upper mold 320 is greater than or equal to the thickness of the annular baffle, that is, the minimum thickness of the bowl-shaped crimping portion is greater than or equal to the thickness of the annular baffle. In this way, while avoiding the problem of overweight of the upper mold 320, the structure can ensure that the shape of the mold cavity does not deform during the hot bending process, and the mold strength also meets the requirements of hot bending. During the preheating process of the glass sheet, the glass sheet continues to soften and deform, and the upper mold 320 falls along the rail through the guide column 321 under the action of its own weight. In this way, the area of ​​the curved surface 322 of the upper mold 320 that abuts against the upper surface of the glass sheet increases, and both are deformed in the direction close to the curved groove 313 of the lower mold 310.

[0048] In this embodiment, the lower mold 310 forms an avoidance surface corresponding to the convex surface of the glass sheet in the second molding area 3132, and the avoidance surface provides a receiving area for the arc surface 322 of the upper mold 320, so that the arc surface 322 of the upper mold 320 can squeeze the concave surface of the molded glass during the hot bending process and position the molded concave surface contour. The upper mold 320 and the lower mold 310 are both made of high temperature resistant graphite material, which can maintain the shape of the upper mold 320 and the lower mold 310 and extend their service life while avoiding the problem of adhesion when taking out the material. Graphite is used to make the mold for hot bending of large-curved optical glass 20 because graphite has the advantages of anti-oxidation, anti-deformation, moderate strength and hardness, not easy to react with glass or stick to it, and good demolding performance. Furthermore, graphite has excellent thermal conductivity under high temperature conditions, which facilitates the rapid conduction of heat to the glass sheet, improves the heating speed and heating effect of the glass sheet, and the graphite molding surface accuracy and surface quality can also meet the hot bending requirements. In addition, graphite raw materials are abundant and cheap, which is conducive to reducing the production cost of the mold.

[0049] The upper mold 320 and the lower mold 310 form a closed system after the mold is closed, which can prevent foreign matter from entering the mold after the mold is closed, causing a poor appearance of the hot bending. In addition, in order to prevent the weight of the upper mold 320 from exceeding the specification, the upper mold 320 is provided with a weight reduction groove 324 corresponding to the first stopper 340 and the second stopper 350, respectively, which can reduce the weight of the upper mold 320 and ensure that a closed system is formed after the mold is closed, so as to prevent suspended particles in the hot bending environment, foreign matter or powder layer formed by graphite shedding from falling into the mold. The first stopper 340 and the second stopper 350 can also be replaced separately when they are damaged or worn, so as to avoid the mold being scrapped together.

[0050] In this solution, since the glass after hot bending needs to be chemically strengthened, the contour of the product after hot bending will change during chemical strengthening. In order to ensure that the size and contour of the large-curved optical glass 20 after hardening meet the user's needs, the mold design can be compensated accordingly according to the change in the contour before and after the product is hardened, so as to reasonably avoid the negative impact of the change in the contour of the large-curved optical glass 20 during chemical strengthening. First, by fixing the relevant process parameters of the large-curved optical glass 20 white sheet and its production equipment, it is ensured that different batches of large-curved optical glass 20 are produced under the same equipment and parameters; secondly, it is ensured that the size and contour of the measured glass and the corresponding hot bending mold are true and reliable; then, the size and contour of the glass required by the user are subtracted from the size and contour of the measured glass, and the deviation between the size and contour of the produced glass and the glass required by the customer is calculated; finally, according to the above calculated deviation, the corresponding mold is compensated accordingly (compensation method: use the size corresponding to the mold, subtract the deviation size) to obtain the mold processing size.

[0051] S3, assemble the insert assembly on the lower mold 310, put the shaped glass sheet 10 into the curved groove 313 of the lower mold 310, and cover the upper mold 320 on the upper part of the shaped glass sheet 10, send the molded graphite mold 30 to the hot bending machine, and perform preheating, molding, slow cooling and fast cooling in sequence. Preferably, the preheating temperature of the graphite mold 30 is between 690℃-810℃, the molding temperature of the graphite mold 30 is between 670℃-795℃, the slow cooling temperature of the graphite mold 30 is between 380℃-680℃, and the fast cooling temperature of the graphite mold is 25℃. During the glass sheet molding process, the glass sheet continues to soften and deform, and the upper mold 320 is pressed by the self-weight of the upper mold 320 and the cylinder of the pressure system. The upper mold 320 continues to fall along the rail through the guide column 321 until the height limit block 330 abuts against the bottom edge of the upper mold 320 to prevent the upper mold 320 from falling further. The softened glass is completely bonded to the arc surface 322 and the inner surface of the curved groove 313 to complete the hot bending of the large-arc optical glass 20, and then undergoes slow cooling and fast cooling processes in sequence to complete the glass shaping.

[0052] In this embodiment, the material model of the glass sheet is Corning 7418, with a thickness of 0.8mm. The glass molding stage passes through three molding workstations in sequence. The temperature of molding workstation 1 is set to 795℃, and the pressure is set to 0.1Mpa / 50S, 0.2Mpa / 50S, and 0.3Mpa / 60S; the temperature of molding workstation 2 is set to 720℃, and the pressure is set to 0.2Mpa / 160S; the temperature of molding workstation 3 is set to 680℃, and the pressure is set to 0.15Mpa / 160S. The pressure also needs to be adjusted according to the type and thickness of the glass. Too much pressure may cause the glass to break, and too little pressure cannot make the glass bend or the contour of the glass bending cannot reach the set value.

[0053] S4. Take out the bent glass sheet and perform CNC machining on the shape of the glass sheet to ensure that the shape and size of the large-curved optical glass after heat bending are finely processed into the shape and size required by the user. The CNC machining parameters are shown in the following table:

[0054]

[0055]

[0056] S5. Take out the glass piece after CNC processing and polish the glass piece comprehensively.

[0057] Specifically, step S5 includes:

[0058] S51. Use a polishing rod to polish the CNC machined trimming area. Step S51 includes: polishing the edge of the glass with a nano-cerium oxide polishing liquid through a polishing rod with a polyurethane polishing pad on the surface to remove defects such as chipped edges and burrs caused by CNC. Specifically, in order to reduce the surface scratches of the product left on the surface of the hot-bent glass during the CNC process, it is necessary to chamfer and polish the edges of the hot-bent glass to simultaneously improve the edge strength of the glass. The parameters for polishing the edges and chamfers are as follows: rough polishing consumables 3M (TD2V), rough polishing spindle speed: 5000rpm, rough polishing feed: 800mm / min; fine polishing consumables 3M (P2), fine polishing spindle speed: 5000rpm, fine polishing feed: 800mm / min.

[0059] S52. Polish the concave and convex surfaces of the glass treated with the polishing rod using a polishing machine and a sponge head.

[0060] Since mold marks are difficult to avoid during the hot bending process, the mold marks on the concave and convex surfaces of the hot bent glass will affect the overall appearance and strength of the glass. In order to reduce and avoid mold marks on the concave and convex surfaces of the hot bent glass, a five-axis polishing machine, a sponge head and a nano-cerium oxide polishing liquid system are used to polish the concave and convex surfaces of the hot bent glass as a whole. First of all, the five-axis polishing machine can polish the concave and convex surfaces of the hot bent glass in all directions without dead angles. The sponge head can keep the abrasive particles in the polishing liquid so that the abrasive can fully contact the product to be polished during the polishing process; the nano-cerium oxide polishing liquid contains abrasives, such as rare earth particles such as cerium oxide. During the polishing process, the glass debris ground off the surface of the glass sheet is also mixed into the polishing liquid, and the glass sheet is polished together with the abrasive in the polishing liquid, and a broken layer is formed on the surface of the glass sheet. The broken layer can be removed by friction with a polyurethane polishing pad to eliminate the mold marks on the glass surface. In this way, while avoiding damage to the glass surface, the mold marks on the glass surface are removed to improve the surface quality of the glass.

[0061] When concave polishing of glass sheets is performed, it is mainly used to remove the mold mark on the concave surface of the hot-bent sample to improve its strength. The fixture for concave polishing is a profiling fixture. The equipment uses a Yujing five-axis polishing machine. The polishing parameters are shown in the following table:

[0062]

[0063]

[0064] The purpose of convex polishing is to remove the mold mark on the convex surface of the hot-bent sample and improve its strength. The fixture for convex polishing is a profiling fixture, and the polishing equipment model is Guangzhou 13.7B. The polishing parameters are shown in the following table:

[0065]

[0066] S6. Chemical hardening and re-polishing are performed on the polished glass sheet in sequence to obtain the target large-curvature optical glass 20. Chemical hardening is used to increase the hardness of the glass and strengthen the glass, while re-polishing is used to remove the residual salt and uneven parts of the hardened glass surface, thereby obtaining a smooth glass product. In this embodiment, the polished glass sheet is chemically strengthened twice, and then the concave surface and convex surface of the glass sheet are re-polished respectively. Specifically, after the concave and convex surfaces of the glass sheet are polished, the first chemical strengthening is performed, and the chemical strengthening conditions are: preheating time: 60±5min, preheating temperature: 330±10℃, first chemical strengthening time: 540±5min; first chemical strengthening temperature: 430±2℃; consumables: 90±2%KNO3(WT%) / 10±2%KNO3NaNO3(WT%) / 0.5±0.1% H2SiO3(WT%). Second chemical strengthening 2: preheating time: 60±1min, preheating temperature: 330±10℃, second chemical strengthening time: 60±1min; second chemical strengthening temperature: 430±2℃; consumables: KNO3≥99.5%(WT%) / H2SiO3≤0.5%(WT%). Concave surface polishing is used to remove the concave and convex points formed on the concave surface of the glass during the hardening process, so as to reduce the surface roughness to Sa<1nm and improve the concave surface strength. The fixture for concave surface polishing is a profiling fixture, and the polishing equipment uses a Yujing five-axis polishing machine. The polishing parameters are shown in the following table:

[0067]

[0068] Convex surface polishing is used to remove the concave and convex points formed on the convex surface of the glass during the hardening process, so that its surface roughness is reduced to Sa<1nm to improve the surface strength. The fixture for convex surface polishing is a profiling fixture, and the model of the polishing equipment is Guangzhou 13.7B. The polishing parameters are shown in the following table:

[0069]

[0070] It should be noted that, in order to improve the quality of hot bending of glass sheets, this embodiment also proposes a large number of assumptions for the current problems of glass sheets and verifies the results through repeated adjustments, as shown in the following table:

[0071]

[0072] The following describes the mold preparation process and the glass hot bending process with reference to specific examples.

[0073] 1) Graphite mold material selection

[0074] The graphite mold of this embodiment is made of POCO graphite raw material (POCO GRAPHITE), and its expansion coefficient is 7.88X10 -6 / ℃, density is 1.77g / cm3 . The physical properties are as follows:

[0075] Particle size (μm) Ash purity (ppm) Shore hardness (HSD) Thermal conductivity W / (m·K) <3 <5 96 60

[0076] 2) Mold design

[0077] The shape of the mold is designed according to the shape of the aforementioned glass piece, and the size of the mold is finally designed according to the actual size of the finished product, combined with the margin of the size to be processed later, the expansion coefficient of the hot-bent glass and many other factors. The glass of this design does not require external force and local heating during hot bending, and the molding can be completed by controlling the temperature and mastering the time.

[0078] 3) CNC processing of molds

[0079] The CNC processing of the mold in this embodiment includes outer shape processing and molding surface processing.

[0080] Among them, the shape processing parameters are as follows:

[0081] Tool Type Tool Model Tool diameter Maximum speed Maximum feed Diamond electric cutting tool D10R / D3R0 Φ10mm / Φ3mm 24000±500RPM 8000±600mm / min

[0082] The molding surface processing parameters are as follows:

[0083] Tool Type Tool Model Tool diameter Maximum speed Maximum feed Diamond electric cutting tool D6R3 / D4R2 Φ0.6mm / Φ0.4mm 24000±500RPM 8000±600mm / min

[0084] 4) Mold forming surface polishing

[0085] The molding surface of the mold after CNC processing is manually polished with 7000# sand to remove the graphite powder suspended on the molding surface to prevent the glass surface from having bad appearance such as bumps and indentations during hot bending. The criterion for qualified molding surface polishing is Sa<120nm.

[0086] 5) Rough grinding of special-shaped glass

[0087] The CNC cut samples were double-sided thinned using a 9um diamond grinding pad and YM-02 polishing liquid to optimize the surface quality of the flat glass. The fixture used was a concave fixture; the single-side removal amount was 0.245mm; the equipment model was Yunnan 13.7B.

[0088]

[0089] 6) CNC processing of glass shape and chamfering

[0090] The purpose of CNC processing of glass shape and chamfer is to fine-tune the shape and size of the cut flat glass into the shape and size required for hot bending. The parameters are as follows: spindle speed: 28000-32000rpm, rough cutting feed: 200mm / min, fine cutting 1 feed: 1000mm / min, fine cutting 2 feed: 800mm / min, rough cutting grinding wheel: 250#; fine cutting 1 grinding wheel: 400#; fine cutting 2 grinding wheel: 800#.

[0091] 7) Fine grinding

[0092] The samples processed by CNC are double-sided polished by white grinding to reduce surface scratches, and the surface quality of the hot-bent flat sheet is optimized. The fixture adopts a concave fixture, and the single-side removal amount of the polishing surface is: 0.02mm. The equipment model is Guangzhou 13.7B.

[0093]

[0094] 8) Hot bending

[0095] i) Wipe and remove foreign matter on the surface of the graphite mold 30 by vacuum adsorption.

[0096] ii) manually placing the cleaned qualified irregularly shaped glass sheet 10 into the lower mold 310 of the graphite mold 30, closing the upper mold 320 and the lower mold 310 until the convex part of the arc surface 322 of the upper mold 320 abuts against the upper surface of the glass sheet under the action of its own weight, and then sending the closed graphite mold 30 to the entrance of the hot bending machine.

[0097] iii) The mold is sent into the hot bending operation chamber filled with nitrogen in the hot bending machine workstation through a push rod.

[0098] iv) The graphite mold 30 carrying the shaped glass sheet 10 is sent out of the hot bending machine after sequentially passing through preheating, forming, slow cooling and cooling processes. In this embodiment, the graphite mold 30 sequentially passes through 6 preheating stations during preheating; sequentially passes through 3 forming stations during forming; sequentially passes through 5 slow cooling stations during slow cooling; and sequentially passes through 7 cooling stations during cooling.

[0099] Since the main factors affecting the hot bending of curved glass include heating temperature, applied pressure, forming time, etc., but the degree of influence of each process parameter is very different, the hot bending process of glass is very complex and nonlinear. During the forming process, if the temperature of the glass in the mold is too high, the glass will melt, and the mold will stick after cooling; if the glass heating temperature is too low, it will cause cold lines, low precision and even breakage after the glass is hot-bent; during the glass cooling stage, if the cooling rate is too fast, the temperature distribution of the glass sheet will be uneven, especially in the thickness direction of the glass sheet. There will be a large temperature difference, and the product will burst during the forming process due to excessive internal thermal stress. To address this problem, this embodiment uses cross-validation and conducts a large number of experiments to obtain a set of optimal hot bending parameters for each workstation, as shown in the table below;

[0100]

[0101]

[0102] It can be seen that the temperature of the graphite mold 30 gradually increases in each preheating workstation, gradually decreases in each workstation in the forming stage, gradually decreases in each workstation in the slow cooling stage, and remains consistent in each workstation in the cooling stage. In this embodiment, the glass hot bending process is to first place the graphite mold 30 containing the glass sheet on the heating plate of the heating station that has reached the preset temperature, and then push the upper heating plate of the hot bending machine downward by the cylinder on the heating station until the upper heating plate contacts the upper surface of the upper mold 320. In this process, the heating station is set isothermally, and the glass sheet in the graphite mold 30 is heated to a viscoelastic state that can be bent and formed by controlling the temperature of the heating plate and the heating time; then the graphite mold 30 is pushed to the first forming station by the lever device in the forming chamber of the hot bending machine, and the double servo motors on the forming station drive the upper heating plate to move downward to slowly apply downward pressure to the graphite mold 30, so that the glass in the viscoelastic state in the graphite mold 30 is filled and formed; the lever device then pushes the graphite mold 30 to the second forming station and the third forming station in turn, and the servo motor continues to apply pressure to the graphite mold 30, so that the glass sheet is kept under pressure in the graphite mold 30 for a period of time, which is conducive to better shaping of the glass; finally, the graphite mold 30 is pushed to the slow cooling and cooling station for cooling until it drops to room temperature.

[0103] In this embodiment, the graphite mold 30 is allowed to enter various workstations with different temperatures one by one, rather than being placed in a single workstation and adjusting the temperature of the workstation. This is to allow the graphite mold 30 to be transferred between adjacent workstations with a smaller temperature difference. The temperature of the graphite mold 30 can change slowly and naturally, so as to avoid a rapid change in the state of the glass sheet caused by a sudden change in the temperature of the graphite mold 30, which may result in untimely release of internal stress in the glass sheet and further affect the performance of the glass.

[0104] v) Open the graphite mold 30 manually, use a vacuum cleaner to clean the mold and glass after the heat bending, and then check the appearance and size of the molded glass.

[0105] By implementing the large-curve optical glass processing technology of the present invention, the glass sheet after heat bending is polished, chemically strengthened and re-polished, and while ensuring the mechanical strength of the glass sheet, the indentations or concave-convex point defects on the surface of the glass sheet caused by heat bending can be removed, thereby improving the mold indentation problem on the product surface; when the glass sheet is fully polished, the scars in the area where the contour of the glass sheet suddenly changes, the chamfers and the body parts are eliminated, and the strength of the area where the contour of the glass sheet suddenly changes and the edge parts is improved; the special-shaped glass sheet 10 is limited by the insert assembly, which can effectively avoid the relative lateral and upward movement of the glass, so that the special-shaped glass sheet 10 can only be affected by the weight of the upper mold 320 and the external air when softening. The pressure of the cylinder deforms downward and replicates the shape of the inner cavity of the mold. Since the mold gap between the upper mold 320 and the lower mold 310 is the thickness of the target large-curvature optical glass 20, and the contour design of the large-curvature optical glass 20 remains unchanged, that is, the area of ​​the large-curvature optical glass 20 remains unchanged, a reasonable thickness design can not only ensure the strength of the glass, but also achieve control of the weight of the glass. In addition, the gravity of the glass and the friction between the glass and the graphite mold can prevent the glass sheet from shifting during the hot bending process. The slow cooling temperature of the graphite mold is between 380℃-680℃ to avoid wrinkles caused by pulling during glass molding, uneven glass thickness and other defects, thereby improving the hot bending yield of the product.

[0106] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0107] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A large-curvature optical glass processing process, characterized in that: The following steps are involved: S1. Cutting the original glass sheet to obtain a special-shaped glass sheet, wherein the special-shaped glass sheet has a runway-shaped structure, wherein two arcuate short side surfaces of the special-shaped glass sheet respectively form a first body-holding limit area, an arcuate long side surface of one side of the special-shaped glass sheet forms a second body-holding limit area, and the middle portion of the arcuate long side surface of the other side of the special-shaped glass sheet is concave to form a nose bridge limit area, and the special-shaped glass sheet is provided with a non-transition area in the middle thereof and a transition area surrounding the non-transition area; S2. Prepare a graphite mold, which includes a lower mold, an upper mold covered on the lower mold by plugging, and an insert assembly detachably mounted on the lower mold, wherein the lower portion of the upper mold is formed with an arc surface that abuts against the upper surface of the special-shaped glass piece, and the shape of the arc surface is adapted to the concave shape of the target large-curvature optical glass; a curved groove for accommodating the special-shaped glass piece is provided in the middle portion of the upper surface of the lower mold, and the inner surface shape of the curved groove is adapted to the convex shape of the target large-curvature optical glass, and the inner surface of the curved groove has a first molding area corresponding to the transition area and a second molding area corresponding to the non-transition area and located below the first molding area; the lower mold has a first direction along the length direction of the lower mold and a second direction along the width direction of the lower mold, and the lower mold The upper surface is provided with a first card slot and a second card slot opened at two opposite sides of the curved groove along the first direction, and a third card slot and a fourth card slot opened at two opposite sides of the curved groove along the second direction. The insert assembly includes two height limiting blocks which are respectively embedded in the first card slot and the second card slot and respectively fit with the two first body-standing limiting areas, a first stopper which is embedded in the third card slot and fits with the second body-standing limiting area, and a second stopper which is embedded in the fourth card slot and fits with the nose bridge limiting area; the height limiting block, the first stopper and the second stopper are respectively provided with an arc surface structure for limiting the position of the special-shaped glass piece and abutting against the body of the special-shaped glass piece, the shape of the arc surface structure is adapted to the body shape of the special-shaped glass piece, and the mold clearance height between the upper mold and the lower mold is the thickness of the target large-arc optical glass; S3, placing the shaped glass piece into the curved groove of the lower mold, and closing the upper mold cover on the upper part of the shaped glass piece, sending the closed graphite mold to the hot bending machine, and performing preheating, molding, slow cooling and fast cooling in sequence; the preheating temperature of the graphite mold is between 690°C and 810°C, the molding temperature of the graphite mold is between 670°C and 795°C, the slow cooling temperature of the graphite mold is between 380°C and 680°C, and the fast cooling temperature of the graphite mold is 25°C; S4, taking out the hot-bent glass sheet, and performing CNC processing and trimming on the shape of the glass sheet; S5, taking out the glass piece after CNC processing and polishing the glass piece comprehensively; S6. Chemically harden and re-polish the polished glass sheet in sequence to obtain the target large-curvature optical glass.

2. The large-curvature optical glass processing process according to claim 1, characterized in that: The second molding area is a concave arc surface structure, the first molding area is a smooth curved surface, and the angle between the first molding area and the first direction or the angle between the first molding area and the second direction is 35°-55°.

3. The large-curvature optical glass processing process according to claim 1, characterized in that: The first stopper and the second stopper are respectively in a T-shaped structure. Two first ear grooves communicating with the third slot are provided on both sides of the slot opening of the third slot. Two second ear grooves communicating with the fourth slot are provided on both sides of the slot opening of the fourth slot.

4. The large-curvature optical glass processing process according to claim 1, characterized in that: A first arc-shaped groove is provided on one side of the height limiting block adjacent to the curved groove; a middle part of a side of the first stopper adjacent to the second body limiting area is raised to form a first raised portion, and a second arc-shaped groove is provided on one side of the first raised portion adjacent to the curved groove; a middle part of a side of the second stopper adjacent to the nose bridge limiting area is raised to form a second raised portion, and a clamping area is formed between the second raised portion and the nose bridge limiting area, and a limiting groove connected to the fourth slot is provided on the upper surface of the lower mold at the clamping area, and a nose bridge abutting block respectively abutting against the second raised portion and the nose bridge limiting area is inserted in the limiting groove, the depth of the limiting groove is less than the height of the nose bridge abutting block, and the shape of the side of the nose bridge abutting block adjacent to the nose bridge limiting area is adapted to the shape of the nose bridge limiting area.

5. The large-curvature optical glass processing process according to claim 1, characterized in that: A plurality of guide pillars protruding from the lower surface of the upper mold are arranged at intervals on the inner side of the lower part of the upper mold, and a plurality of clamping rails for slidingly embedding the guide pillars in a one-to-one correspondence are arranged on the upper surface of the lower mold.

6. The large-curvature optical glass processing process according to claim 1, characterized in that: The upper surface of the upper mold is provided with a hollow structure and a plurality of protrusions, and the weight of the upper mold is 1.33-1.46 kg.

7. The large-curvature optical glass processing process according to claim 1, characterized in that: Step S5 includes: S51, polishing the CNC machined finishing area using a polishing rod; S52. Polish the concave and convex surfaces of the glass treated with the polishing rod using a polishing machine and a sponge head.

8. The large-curvature optical glass processing process according to claim 7, characterized in that: Step S51 includes: The edge of the glass is polished by using a polishing rod with a polyurethane polishing pad on the surface and nano-cerium oxide polishing liquid.

Citation Information

Patent Citations

  • Vacuum mold apparatus, systems, and methods for forming curved mirrors

    CN111630008A

  • Glass hot bending mold and glass hot bending forming method

    CN114455818A

  • Laser cutting method for three-dimensional curved glass

    CN116282875A

  • Hot bending forming process for glass rear cover of electronic equipment

    CN118026507A