Lithium slag-based geopolymer cementing material and preparation method thereof
By activating lithium slag and combining with other materials, the lithium slag base polymer gelling material is prepared, which solves the problem of low reactivity of lithium slag, and realizes the efficient utilization of lithium slag and environmentally friendly low-carbon building materials production, providing the Satisfied mechanical properties and carbon emission reduction effect.
Patent Information
- Application Number
- CN202411007808.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-15
AI Technical Summary
Lithium slag generates a large amount of production, and its simple accumulation or landfill causes harm to the environment. Its reaction activity is low when preparing geological polymers, affecting performance, and limiting its large-scale utilization.
By activating lithium slag, increasing its specific surface area, combining it with ore powder, fly ash, semi-water gypsum and other materials, adding compound admixtures to prepare lithium slag base polymer cementitious material to replace traditional cement production of concrete etc. to reduce carbon emissions and energy consumption.
It effectively improves the activity of lithium slag, reduces carbon emissions and energy consumption, realizes efficient utilization of lithium slag, provides satisfactory mechanical properties, and can partially replace cement for the production of green and low-carbon building materials.
Smart Images

Figure CN118955018A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of comprehensive utilization of solid waste and low-carbon gelling materials, and in particular to a lithium slag-based polymer gelling material and a preparation method thereof. Background Art
[0002] Lithium has the characteristics of low density and active chemical properties. It is widely used in electronic equipment, new energy vehicles and other fields. It is called the energy metal of the 21st century. With the growth of consumer markets such as electronic products and power batteries (new energy vehicle field), the total consumption of lithium will become larger and larger. A large amount of lithium slag will be produced in the production process of lithium or lithium salt. For every ton of lithium salt produced, 8-10 tons of lithium slag will be produced. The waste slag produced by preparing lithium or lithium salt by different preparation methods accounts for more than 90% of the total mineral amount. The production of a large amount of lithium slag has always troubled lithium production companies. Lithium slag is the waste slag produced in the process of extracting lithium and its compounds from lithium-containing ores. The main chemical components of lithium slag are SiO2 and A12O3. It is a high-quality aluminum silicate mineral, but a certain amount of sulfide and harmful elements remain. Simple accumulation or landfill will cause harm to the surrounding soil and groundwater. The resource utilization of lithium slag is mainly concentrated in concrete, cement mortar, ceramics, molecular sieves, etc., but its usage is only 20%, which is very limited, seriously restricting its large-scale utilization.
[0003] Geopolymer is a type of aluminum silicate gelling material, which belongs to a new type of green building material. Geopolymer has excellent mechanical properties, high temperature resistance and corrosion resistance. It can replace silicate cement in the field of building materials, and also has good performance in the fields of heavy metal waste and nuclear waste consolidation, porous adsorption materials, high-performance composite materials, etc. The content of Si02 and A120 in lithium slag reaches 70%, which meets the requirements of raw material components of geopolymer, but contains more gypsum, resulting in low reaction activity, easy to form false solidification, and seriously affecting the performance of geopolymer. Therefore, lithium slag cannot be directly used to prepare geopolymer. At present, the glass phase content in lithium slag is increased by calcination heat treatment (500-700℃), and better reaction activity in alkaline solution is obtained, so as to prepare geopolymer. Even so, it is still necessary to add activated white carbon black, fly ash or steel slag to adjust the silicon-aluminum ratio and sodium-aluminum ratio in the raw material components.
[0004] Based on this, a green and low-carbon building material that can effectively utilize lithium slag-based polymer cementitious materials to replace cement for the production of concrete, aerated blocks and prefabricated structures is urgently needed in the industry. Summary of the invention
[0005] In order to make full use of lithium slag resources, the present invention proposes a hydraulic lithium slag-based polymer cementitious material and a preparation method thereof, which can efficiently utilize lithium slag resources while reducing pollution. Compared with the traditional cement production process of two grindings and one burning, the prepared lithium slag-based polymer cementitious material can reduce carbon emissions by about 80% and energy consumption by 60%, and has satisfactory mechanical properties.
[0006] The present invention is achieved by the following technical means:
[0007] A lithium slag-based polymer gelling material comprises the following raw materials in proportions by weight:
[0008] 30-70 parts of activated lithium slag, 10-50 parts of mineral powder, 5-20 parts of fly ash, 5-15 parts of hemihydrate gypsum, and 0.5-2 parts of compound admixture.
[0009] Furthermore, the lithium slag-based polymer gelling material comprises the following raw materials in proportion by weight:
[0010] 50 parts of activated lithium slag, 30 parts of mineral powder, 9 parts of fly ash, 10 parts of hemihydrate gypsum, and 1 part of compound admixture.
[0011] Furthermore, the mineral powder has an activity of 95.
[0012] The present invention also discloses a method for preparing a lithium slag-based polymer gelling material, comprising the following steps:
[0013] Activation method:
[0014] (1) Lithium slag activation treatment: triisopropanolamine and limestone are added to the lithium slag for ball milling to increase the specific surface area of the lithium slag from 150-200m 2 / kg increased to 500-700m 2 / kg, and activated lithium slag is obtained for later use;
[0015] (2) Preparation of lithium slag-based polymer cementitious material: Add mineral powder, fly ash and hemihydrate gypsum to activated lithium slag, mix well and then add compound admixture to obtain a lithium slag-based polymer cementitious material.
[0016] Furthermore, in step (1), the amount of triisopropanolamine used is 0.1% of the mass of the lithium slag; and the amount of limestone used is 3% of the mass of the lithium slag.
[0017] Furthermore, in step (1), the ball milling speed is 25 r / min and the ball milling time is 45 min.
[0018] Furthermore, the compound admixture in step (2) is prepared from the following raw materials:
[0019] Calculate the mixture by mass by mixing 0.2 parts of sodium hydroxide, 0.2 parts of sodium silicate and 0.6 parts of quicklime evenly.
[0020] The invention also discloses a lithium slag-based polymer gelling material prepared according to any one of the above preparation methods.
[0021] The present invention also discloses a use of any of the above-mentioned lithium slag-based polymer cementitious materials in the preparation of concrete, aerated blocks or prefabricated low-carbon building materials.
[0022] The beneficial effects of the present invention are:
[0023] 1. Since the activity of lithium slag cannot meet the demand, the present invention first activates the lithium slag to improve the working performance of the lithium slag. The activation method is to add triisopropanolamine and limestone as grinding aids to increase the fineness of the lithium slag, thereby increasing the specific surface area of the lithium slag from 150-200m 2 / kg increased to 500-700m 2 / kg, which greatly improves the rate of gelation reaction and makes the activity of lithium slag reach the utilization requirement.
[0024] 2. Lithium slag contains abundant chemical components such as SiO2, Al2O3, CaO, Na2O, K2O, etc., among which the silicon-aluminum ratio is about 0.4, so lithium slag has potential volcanic ash activity. The silicon-aluminum molar ratio of lithium slag is close to 2:1. Minerals containing silicon and aluminum can undergo geopolymerization reaction with alkaline activators to generate aluminosilicate gel with a three-dimensional network structure. This gel has good adhesion and durability. Therefore, lithium slag-based polymer cementitious materials can be prepared through this property of geopolymer. It is well known that the production process of silicate cement, a commonly used cementitious material, will emit a large amount of CO2. Compared with the traditional cement production process of two grinding and one burning, the preparation of geopolymer cementitious materials with lithium slag can reduce carbon emissions by about 80% and energy consumption by 60%, and at the same time have satisfactory mechanical properties. Lithium slag-based polymer cementitious materials can partially replace cement for the production of green and low-carbon building materials such as concrete, aerated blocks and prefabricated structures. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The lithium slag walkway brick prepared in Example 1 of the present invention;
[0026] Figure 2 The lithium slag insulation building block is prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0027] The present invention provides a large-volume lithium slag waste comprehensive utilization technology and its implementation method. In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0028] Example 1
[0029] A lithium slag-based polymer gelling material and a preparation method thereof:
[0030] 50 parts of activated lithium slag, 30 parts of 95 mineral powder, 9 parts of fly ash, 10 parts of hemihydrate gypsum, and 1 part of compound admixture.
[0031] (1) Lithium slag activation treatment: 0.1% triisopropanolamine and 3% limestone were added to the lithium slag for ball milling at a speed of 25 r / min for 45 min to increase the specific surface area of the lithium slag from 150-200 m 2 / kg increased to 500-700m 2 / kg, and activated lithium slag is obtained for later use;
[0032] (2) Preparation of compound admixture: 0.2 parts of sodium hydroxide, 0.2 parts of sodium silicate and 0.6 parts of quicklime are mixed evenly to obtain a compound admixture for use;
[0033] (3) Preparation of lithium slag-based polymer cementitious material: adding mineral powder, fly ash and hemihydrate gypsum to activated lithium slag, mixing evenly and then adding compound admixture to obtain a lithium slag-based polymer cementitious material.
[0034] The performance of the lithium slag-based polymer cementitious material obtained in Example 1 is as follows: the standard consistency measured by a Vicat instrument is a water-cement ratio of 0.38, that is, the mass ratio of cementitious material: water is 1 part:0.38 parts; the initial setting time measured according to the standard "Cement Setting Time Test Method" is 1 hour and 20 minutes, and the final setting time is 2 hours and 5 minutes; according to the standard "Cement Mortar Strength Test Method", a 40mm*40mm*160mm mortar test block is prepared, and the 3-day flexural strength of the test block is measured to be 2.75 MPa, the compressive strength is 19.4 MPa, the 28-day flexural strength is 5.8 MPa, and the compressive strength is 44.5 MPa.
[0035] Compared with the national standard GB175-2023 "General Portland Cement", the lithium slag-based polymer cementitious material prepared in this example meets the compressive strength requirements of composite Portland cement with a grade of 42.5, that is, greater than 17 MPa in 3 days and greater than or equal to 42.5 MPa in 28 days; the flexural strength is slightly worse. The standard requires a three-day strength of 4.0 MPa, which is 2.75 MPa in this example, and requires a 28-day strength of 6.5 MPa, which is 5.8 MPa in this example. Therefore, the cementitious material prepared in this example can only partially replace Portland cement to prepare building materials.
[0036] In this example, the amount of lithium slag used is 50% of the total mass. The hydraulic cementitious material obtained can meet the strength requirements of many building materials, such as walkway bricks, masonry mortar and aerated blocks.
[0037] Example 2
[0038] A lithium slag-based polymer gelling material and a preparation method thereof:
[0039] The preparation method is the same as in Example 1, except that the formula is changed, specifically:
[0040] 60 parts of activated lithium slag, 20 parts of 95 mineral powder, 9 parts of fly ash, 10 parts of hemihydrate gypsum, and 1 part of compound admixture.
[0041] The performance of the lithium slag-based polymer cementitious material obtained in Example 2 is as follows: the standard consistency measured by a Vicat instrument is a water-cement ratio of 0.41, that is, the mass ratio of cementitious material: water is 1 part:0.38 parts; the initial setting time measured according to the standard "Cement Setting Time Test Method" is 45 minutes, and the final setting time is 1 hour and 25 minutes; according to the standard "Cement Mortar Strength Test Method", a 40mm*40mm*160mm mortar test block is prepared, and the 3-day flexural strength of the test block is 3.7 MPa, the compressive strength is 29.5 MPa, the 28-day flexural strength is 5.0 MPa, and the compressive strength is 36.8 MPa.
[0042] Compared with the national standard of silicate cement, the lithium slag-based polymer cementitious material prepared in this example meets the compressive strength requirements of composite silicate cement with the label of 32.5, that is, greater than 12 MPa in 3 days and greater than or equal to 32.5 MPa in 28 days; the flexural strength is slightly worse, the standard requires a three-day strength of 3.0 MPa, and this example is 2.15 MPa, and the standard requires a 28-day strength of 5.5 MPa, and this example is 5.0 MPa. Therefore, the compressive strength index of the cementitious material prepared in this example meets the requirements of 32.5 cement, and the flexural strength is slightly lower than the minimum requirement of 32.5 cement.
[0043] In this example, the amount of lithium slag used is 60% of the total mass, and the utilization rate of lithium slag is 10% higher than that in Example 1. The obtained hydraulic cementitious material is slightly inferior to 32.5 silicate cement, but it can still meet the strength requirements of many building materials, such as aerated blocks, masonry mortars, and curbstones.
[0044] Embodiment 3 (best strength)
[0045] A lithium slag-based polymer gelling material and a preparation method thereof:
[0046] The preparation method is the same as in Example 1, except that the formula is changed, specifically:
[0047] 35 parts of activated lithium slag, 45 parts of 95 mineral powder, 9 parts of fly ash, 10 parts of hemihydrate gypsum, and 1 part of compound admixture.
[0048] The performance of the lithium slag-based polymer cementitious material obtained in Example 3 is as follows: the standard consistency measured by a Vicat instrument is a water-cement ratio of 0.35, that is, the mass ratio of cementitious material: water is 1 part:0.35 parts; the initial setting time measured according to the standard "Cement Setting Time Test Method" is 3 hours and 20 minutes, and the final setting time is 4 hours and 35 minutes; according to the standard "Cement Mortar Strength Test Method", a 40mm*40mm*160mm mortar test block was prepared, and the 3-day flexural strength of the test block was measured to be 3.7 MPa, the compressive strength was 29.4 MPa, the 28-day flexural strength was 6.2 MPa, and the compressive strength was 63.9 MPa.
[0049] According to the national standard GB175-2023 "General Portland Cement", the lithium slag-based polymer cementitious material prepared in this example meets the compressive strength requirements of composite Portland cement with a grade of 52.5, that is, greater than 22 MPa in 3 days and greater than or equal to 52.5 MPa in 28 days; the flexural strength is close to the requirements of 42.5 cement. The standard requires a three-day strength of 4.0 MPa, which is 3.7 MPa in this example, and requires a 28-day strength of 6.5 MPa, which is 6.2 MPa in this example. The strength performance of the lithium slag-based hydraulic cementitious material prepared in this example is improved compared with Examples 1 and 2, so the scope of use is further expanded.
[0050] In this example, the amount of lithium slag used is 35% of the total mass. The utilization rate of lithium slag is low, but the hydraulic cementitious material obtained has good performance and can meet the strength requirements of most building materials, such as curbstones, self-leveling mortar and grouting materials.
[0051] Example 4
[0052] A lithium slag-based polymer gelling material and a preparation method thereof:
[0053] The preparation method is the same as in Example 1, except that the formula is changed, specifically:
[0054] 70 parts of activated lithium slag, 10 parts of 95 mineral powder, 9 parts of fly ash, 10 parts of hemihydrate gypsum, and 1 part of compound admixture.
[0055] In this example, the amount of lithium slag used is 70% of the total mass, and the utilization rate of lithium slag is 20% higher than that in Example 1. The obtained lithium slag geopolymer cementitious material is slightly inferior to 32.5 silicate cement, but it can still meet the strength requirements of many building materials, such as aerated blocks, masonry mortars, partition boards and other products.
[0056] Compared with the national standard of silicate cement, the lithium slag-based polymer cementitious material prepared in this example basically meets the compressive strength requirements of composite silicate cement with the label of 32.5, that is, greater than 12 MPa in 3 days, 12.9 MPa in this example, greater than or equal to 32.5 MPa in 28 days, 30.3 MPa in this example is slightly worse; the flexural strength is slightly worse, the standard requires a strength of 3.0 MPa in three days, 1.85 MPa in this example, and the standard requires a strength of 5.5 MPa in 28 days, 4.8 MPa in this example. Because the utilization rate of lithium slag of the hydraulic cementitious material prepared in this example reaches 70%, which is relatively high, it is acceptable to be close to the standard requirements of 32.5 cement.
[0057] Example 5
[0058] A lithium slag-based polymer gelling material and a preparation method thereof:
[0059] The preparation method is the same as in Example 1, except that the formula is changed, specifically:
[0060] 50 parts of activated lithium slag, 30 parts of 95 mineral powder, 9.5 parts of fly ash, 10 parts of hemihydrate gypsum, and 0.5 parts of compound admixture.
[0061] Compared with Example 1, the amount of compound admixture is reduced in this example. Compared with the national standard of silicate cement, the lithium slag-based polymer cementitious material prepared in this example fully meets the compressive strength requirements of composite silicate cement with the label of 32.5, that is, greater than 12 MPa in 3 days, 13.4 MPa in this example, and greater than or equal to 32.5 MPa in 28 days, 37.9 MPa in this example; the flexural strength is slightly worse, the standard requires a strength of 3.0 MPa in three days, 1.65 MPa in this example, and the standard requires a strength of 5.5 MPa in 28 days, 5.1 MPa in this example. Because the amount of admixture used in this example is less, the cost performance is relatively good, and its strength can be close to the standard requirements of 32.5 silicate cement, which can also meet the needs of many building materials products.
[0062] Comparative Example 1
[0063] A lithium slag-based polymer gelling material and a preparation method thereof:
[0064] The preparation method is the same as in Example 1, except that the formula is changed, specifically:
[0065] 50 parts of non-activated lithium slag, 95 parts of mineral powder, 1 part of fly ash, 10 parts of hemihydrate gypsum, and 1 part of compound admixture.
[0066] In this comparative example, non-activated lithium slag is used to replace activated lithium slag. The strength is almost non-existent after 3-7 days, and the strength after 28 days is also relatively poor, with a compressive strength of only 3.6 MPa. At this time, the lithium slag can only be used as a filling material.
[0067] Comparative Example 2
[0068] A lithium slag-based polymer gelling material and a preparation method thereof:
[0069] The preparation method is the same as in Example 1, except that the formula is changed, specifically:
[0070] 80 parts of activated lithium slag, 9 parts of fly ash, 10 parts of hemihydrate gypsum, and 1 part of compound admixture.
[0071] In this comparative example, no mineral powder was added. As a result, it was found that the water demand increased, the strength was poor, the setting time was too short, and the initial setting time was only 25 minutes, resulting in a short working time. In addition, the 28-day compressive strength was also relatively low, only 16.8 MPa. It can be seen that there are mineral components in the mineral powder that stimulate the activity of lithium slag and react with lithium slag. The lack of these components has a greater impact on the material properties.
[0072] Comparative Example 3
[0073] A lithium slag-based polymer gelling material and a preparation method thereof:
[0074] The preparation method is the same as in Example 1, except that the formula is changed, specifically:
[0075] 50 parts of activated lithium slag, 39 parts of 95 mineral powder, 10 parts of hemihydrate gypsum, and 1 part of compound admixture.
[0076] In this comparative example, fly ash is not added, and the flexural and compressive strengths are reduced to a certain extent. The 28-day compressive strength of the prepared cementitious material is 32.6 MPa, which is 11.6 MPa lower than the compressive strength of 44.2 MPa in Example 1. Converted into percentage strength, it is reduced by 26.3%, indicating that the addition of fly ash in the formula greatly improves the material performance.
[0077] Comparative Example 4
[0078] The preparation method is the same as in Example 1, except that the formula is changed, specifically:
[0079] 50 parts of activated lithium slag, 30 parts of 95 mineral powder, 9 parts of fly ash, 10 parts of dihydrate gypsum, and 1 part of compound admixture.
[0080] This comparative example does not add hemihydrate gypsum, but uses dihydrate gypsum instead, which leads to a significant decrease in early strength. The three-day compressive strength is 2.5 MPa, which is 87.1% lower than the three-day compressive strength of 19.4 MPa in Example 1. This shows that hemihydrate gypsum has a relatively large effect on early strength. In addition, after using dihydrate gypsum, the initial setting time is 8 hours and 35 minutes, which is significantly longer than 1 hour and 20 minutes in Example 1; in addition, the 28-day compressive strength of the material in Comparative Example 4 is 36.6 MPa, which is lower than 44.2 in Example 1. Therefore, from the perspective of material performance, hemihydrate gypsum is better than dihydrate gypsum. However, it should be noted that the performance of the cementitious material prepared using dihydrate gypsum is also of certain use value in filling materials.
[0081] Comparative Example 5
[0082] The preparation method is the same as in Example 1, except that the formula is changed, specifically:
[0083] 50 parts of activated lithium slag, 30 parts of 95 ore powder, 10 parts of fly ash, and 10 parts of hemihydrate gypsum.
[0084] This comparative example does not add compound admixtures, because there is no activator, resulting in a slow reaction, and the initial setting time is 18 hours and 45 minutes, which is too long compared with the initial setting time of 1 hour and 20 minutes in Example 1, which greatly limits the practical application of this cementitious material; and because no admixture is added, the gelling reaction is insufficient, and the experimental data show that the 28-day compressive strength of the material in Comparative Example 5 is only 15.6 MPa, which is 64.7% lower than 44.2 MPa in Example 1. Through the above experiments, it can be concluded that the compound admixture in the cementitious material is an important component, and if it is missing, it will have a greater adverse effect on the material performance.
[0085] Test results summary:
[0086] The performance of the lithium slag-based polymer gelling materials obtained in Examples 1 to 5 and Comparative Examples 1 to 5 was measured. The measurement standards used in the present invention are as follows:
[0087] (1) Standard consistency: Standard Test Methods for Cement and Its Products (GB / T176-2008);
[0088] (2) Setting time: GB / T9414-2008 Test method for setting time of cement;
[0089] (3) Strength: GB / T17671-1999 “Test method for strength of cement mortar”;
[0090] The specific results are shown in Table 1:
[0091] Table 1
[0092]
[0093]
[0094] According to the results in Table 1, the lithium slag-based polymer cementitious material prepared by the process and formula of the present invention is significantly better than the control group in terms of the comprehensive performance of setting time, 3d strength and 28d strength.
[0095] Application Example 1
[0096] Industrial trial production of walkway bricks:
[0097] The produced walkway bricks are as follows Figure 1 As shown: 10 parts of the lithium slag-based polymer cementitious material in Example 1 are added, and the other 90 parts are sand and gravel aggregates and mixing water. Walkway bricks are prepared after being molded under 150 tons of pressure. After testing, the prepared walkway bricks have a compressive strength of 28 MPa in 3 days and a compressive strength of 60 MPa in 28 days.
[0098] Application Example 2
[0099] Industrial trial production of self-insulating blocks
[0100] Homogeneous self-insulating blocks such as Figure 2 As shown: 60 parts of the lithium slag-based polymer cementitious material prepared in Example 1 and the other 40 parts of polystyrene particles, rubber powder and mixing water are added to prepare a homogeneous self-insulating building block with a density of 0.48 kg / L, a 28-day compressive strength of 2.6 MPa and a thermal conductivity of 0.1 W / (m·K).
[0101] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.
Claims
1. A lithium slag-based polymer gelling material comprising: 30-70 parts of activated lithium slag, 10-50 parts of mineral powder, 5-20 parts of fly ash, 5-15 parts of hemihydrate gypsum, and 0.5-2 parts of compound admixture.
2. The lithium slag-based polymer gelling material according to claim 1, wherein: 50 parts of activated lithium slag, 30 parts of mineral powder, 9 parts of fly ash, 10 parts of hemihydrate gypsum, and 1 part of compound admixture.
3. A method for preparing the lithium slag-based polymer gelling material according to claim 1 or 2, comprising: (1) Lithium slag activation treatment: adding triisopropanolamine and limestone to the lithium slag for ball milling to obtain activated lithium slag for later use; (2) Preparation of lithium slag-based polymer cementitious material: Add mineral powder, fly ash and hemihydrate gypsum to activated lithium slag, mix well and then add compound admixture to obtain a lithium slag-based polymer cementitious material.
4. The preparation method according to claim 3, wherein: The amount of triisopropanolamine used in step (1) is 0.1% of the mass of the lithium slag; the amount of limestone used is 3% of the mass of the lithium slag.
5. The preparation method according to claim 3, wherein: The ball milling speed in step (1) is 25 r / min and the ball milling time is 45 min.
6. The preparation method according to claim 3, wherein: The compound admixture in step (2) is prepared from the following raw materials: Calculate the mixture by mass by mixing 0.2 parts of sodium hydroxide, 0.2 parts of sodium silicate and 0.6 parts of quicklime evenly.
7. A lithium slag-based polymer gelling material obtained according to the preparation method according to any one of claims 3 to 6.
8. Use of the lithium slag-based polymer cementitious material according to any one of claims 1, 2 or 7 in the preparation of concrete, aerated blocks or prefabricated low-carbon building materials.
Citation Information
Cited By
Acid-excited lithium slag-based cementing material and preparation method thereof
CN119683879A
High-doping-amount lithium slag-based geopolymer and preparation method thereof
CN120136467A
Comprehensive recovery method of lithium slag
CN120714773A
Lithium slag-based low-carbon cementing material as well as preparation method and application thereof
CN122355676A