Hydrogenated conjugated diene and bio-based terpene multi-element random copolymer as well as preparation method and application thereof
Through the copolymerization and hydrogenation of conjugated dienes and bio-based terpenes, the problems of insufficient raw material supply and gap in hydrogenation technology in the POE industry are solved, and hydrogenated copolymers with high hydrogenation degree have excellent mechanical properties and cost reduction advantages. Alternative to traditional POE materials.
Patent Information
- Application Number
- CN202411002687.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-25
AI Technical Summary
The POE industry faces the problems of insufficient raw material supply and immature polymerization process, especially the hydrogenation technology of bio-based terpenes such as myrene and farnesene is less researched, and there is a lack of effective catalytic systems and hydrotreating processes.
Provide a polyvariate random copolymer of hydrogenated conjugated diene and bio-based terpene and its preparation method. By copolymerizing and hydrogenating conjugated diene and bio-based terpene, it adopts Ziegler-Natta hydrogenation reaction system or metallocene hydrogenation reaction System to produce hydrogenated polymers with POE properties.
It has achieved a high degree of hydrogenation and has excellent weather resistance, mechanical strength and ductility, replaced traditional POE materials, reduced raw material costs and operating complexity, and broken the monopoly position of POE products.
Smart Images

Figure CN118955801A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of olefin catalytic polymerization and hydrogenation, and specifically relates to a hydrogenated conjugated diene and bio-based terpene multi-component random copolymer and a preparation method and application thereof. Background Art
[0002] POE generally refers to a copolymer of ethylene and propylene or other alpha olefins (such as 1-octene, etc.), which is polymerized in solution using a metallocene catalyst system at a temperature above the melting point of the polymer. Compared with general polyolefins, POE has a longer side chain on the molecular chain, resulting in the coexistence of crystalline and amorphous phases, resulting in unique processing characteristics - while reflecting the high elasticity of rubber, it can be processed and formed using the technology of thermoplastics. At the same time, from the perspective of the bonding of POE itself, because most of the molecular chain is composed of saturated single bonds, it has excellent aging resistance and corrosion resistance.
[0003] At present, the demand for POE in downstream applications is strong, showing a trend of diversification, differentiation and high-end development, mainly in the fields of photovoltaic films, automotive materials, packaging, foamed shoe materials, household appliances and wires and cables. However, the development of POE-related industries still faces the problems of insufficient raw material supply and immature polymerization process, and solutions are urgently needed.
[0004] 1,3-Diene is a class of olefin monomers with a wide range of sources and sufficient supply, and some of them, such as myrcene and farnesene, are renewable resources. At present, the relevant catalytic polymerization technology is relatively mature, but the application research of the hydrogenated products of polymers is not systematic and has not yet formed a major research hotspot, especially for bio-based terpenes such as myrcene and farnesene. There are few reports on the hydrogenation technology containing these two monomers. In view of the above problems, it is necessary to develop a catalytic system and its subsequent catalytic hydrogenation process to obtain a hydrogenated polymer with POE properties using 1,3-diene. Summary of the invention
[0005] The purpose of the present invention is to solve the shortage of raw material supply encountered by the POE industry and fill the gap in the research related to 1,3-diene hydrides, and to provide a hydrogenated conjugated diene and bio-based terpene multi-random copolymer and its preparation method and application.
[0006] The technical solution of the present invention is as follows:
[0007] One of the purposes of the present invention is to provide a hydrogenated conjugated diene and bio-based terpene multi-random copolymer, wherein the copolymer is formed by copolymerizing and hydrogenating at least one of the conjugated diene monomers and at least one of the bio-based terpene monomers, wherein the conjugated diene monomer has a general formula of C n H 2n-2, n≥4, the general formula of bio-based terpene monomer is (C5H8) n , n≥2, the molar content of conjugated diene-based polymerization units is 10% to 90%, the molar content of bio-based terpene-based polymerization units is 10% to 90%, and the degree of hydrogenation is 90% to 99.9%.
[0008] Preferably, the conjugated diene monomers include 1,3-butadiene, isoprene, 1,5-hexadiene, 1,7-octadiene, and the bio-based terpene monomers include limonene, α-pinene, β-pinene, α-myrcene, β-myrcene, α-farnesene, β-farnesene.
[0009] Further preferably, the conjugated diene monomer is isoprene or 1,3-butadiene, and the bio-based terpene monomer is β-myrcene or β-farnesene.
[0010] Preferably, the copolymer has a number average molecular weight of 10,000 to 500,000 g / mol, a molecular weight distribution of 1.0 to 5.0, a glass transition temperature of -80°C to 20°C, a Shore A hardness of >40, a rebound elastic modulus of >20%, an elongation at break of >600%, a tear strength of >20 N / mm, and a volume resistivity of >0.6×10 18 Ω.cm, melting point 55℃~80℃, melt index 60~80g / 10min, heat deformation temperature>125℃, light transmittance at 380-1100nm>89%, water vapor transmittance<3.5%, low temperature notched impact strength (-30℃)>59kJ / m 2 , Izod notch impact strength>70kJ / m 2 .
[0011] Further preferably, the molecular weight distribution of the copolymer is 1.4 to 3.1, the degree of hydrogenation is 95% to 99%, the glass transition temperature range is -68°C to -25°C, the Shore A hardness is greater than 52, the rebound elastic modulus is greater than 23%, the elongation at break is greater than 650%, the tear strength is greater than 27N / mm, and the volume resistivity is greater than 0.76×10 18 Ω.cm, melting point 62℃~69℃, melt index 66~76g / 10min, heat deformation temperature>132℃, light transmittance at 380-1100nm>92%, water vapor transmittance<2.8%, low temperature notched impact strength (-30℃)>62kJ / m 2 , Izod notch impact strength>76kJ / m 2 .
[0012] The second object of the present invention is to provide a method for preparing a hydrogenated conjugated diene and bio-based terpene multi-random copolymer, the method being carried out according to the following steps:
[0013] (1) preparing a multi-component random copolymer by copolymerizing a conjugated diene monomer and a bio-based terpene monomer;
[0014] (2) The multi-component random copolymer is dissolved in a solvent to obtain a copolymer solution, and then hydrogenated by a Ziegler-Natta hydrogenation reaction system or a metallocene hydrogenation reaction system to obtain a hydrogenated conjugated diene and bio-based terpene multi-component random copolymer.
[0015] Preferably, the preparation of the multi-component random copolymer in step (1) is carried out by anionic polymerization, cationic polymerization, free radical polymerization or coordination polymerization. More preferably, it is coordination polymerization, anionic polymerization or free radical polymerization. More preferably, it is coordination polymerization or anionic polymerization.
[0016] Preferably, the coordination polymerization method includes iron coordination polymerization, Zignata-type catalyst system polymerization, cationic lutetium coordination complex polymerization with β-diaminosulfonate as ligand, rare earth lanthanum catalyst polymerization system polymerization, [OSSO] type titanium complex polymerization, half sandwich scandium complex polymerization, and cobalt catalyst system polymerization.
[0017] When the preparation of the multi-component random copolymer adopts the iron coordination polymerization method, the specific steps are: under anhydrous and oxygen-free conditions, add an iron catalyst, a co-catalyst, a conjugated diene monomer, a bio-based terpene monomer and a solvent into a reactor, and stir the polymerization reaction at -30°C to 100°C for 10min to 120min. More preferably, the reaction temperature is -20°C to 30°C, and the reaction time is 30min.
[0018] Preferably, the iron catalyst is any one of the following structural formulas:
[0019]
[0020] When the multi-component random copolymer is prepared by anionic polymerization, the specific steps are: under anhydrous and oxygen-free conditions, an organic alkali metal is used as an initiator to initiate copolymerization of a conjugated diene monomer and a bio-based terpene monomer;
[0021] Alternatively, under anhydrous and oxygen-free conditions, an organic alkali metal is used as an initiator and an organic aluminum compound is used as a co-catalyst to initiate the copolymerization of a conjugated diene monomer and a bio-based terpene monomer.
[0022] Preferably, the organic alkali metal is one or more of n-butyllithium, sec-butyllithium, tert-butyllithium, lithium tert-butoxide, methyllithium, ethyllithium, n-propyllithium, isopropyllithium, phenyllithium, benzyllithium, and naphthalenelithium; the organic aluminum compound can be abbreviated as AB, wherein A represents one or more of trimethylaluminum, triethylaluminum, triisobutylaluminum, diethylaluminum monochloride, ethylaluminum dichloride, or sesquiethylaluminum chloride, and B represents one or more of 2,6-di-tert-butyl-p-cresol, table 2,6-di-tert-butylphenol, 2-tert-butylphenol, or 2,6-di-tert-butyl-4-ethylphenol.
[0023] Preferably, the reaction temperature is -50°C to 70°C, and the reaction time is 10 min to 360 min; more preferably, the reaction temperature is 30°C, and the reaction time is 30 min.
[0024] Preferably, the concentration of the copolymer solution in step (2) is 10 wt %.
[0025] Preferably, the solvent of the copolymer solution in step (2) is one or more of toluene, xylene, n-hexane and cyclohexane.
[0026] Preferably, in step (2), when a Ziegler-Natta hydrogenation reaction system is used, the specific process of hydrogenation is:
[0027] Under an argon atmosphere, the copolymer solution, catalyst and co-catalyst are added in sequence to a dry high-temperature reactor. The gas in the reactor is replaced three times with hydrogen. The reactor speed is adjusted to 100-1000 rpm, the hydrogenation reaction pressure is 1-5 MPa, the temperature is increased to 95°C-120°C, and the reaction is carried out for 1-5 hours.
[0028] Further preferably, the catalyst is one or more of nickel sulfate, nickel chloride, nickel nitrate or nickel cyclohexaneate; the co-catalyst is an organic metal compound of a metal from Group IA to Group IIIA, more preferably one or more of trimethylaluminum, tri-n-butylaluminum, triisobutylaluminum, triethylaluminum, diethylaluminum monochloride, ethylaluminum dichloride, and diisobutylaluminum hydride.
[0029] More preferably, the mass ratio of the copolymer to the catalyst in the copolymer solution is (1-500):1; and the molar ratio of the catalyst to the co-catalyst is 1:(1-20).
[0030] Preferably, the metallocene hydrogenation reaction system in step (2) comprises a bis(titanocenes) / lithium hydride / aromatic ester system, a bis(titanocenes) or mono(titanocenes) / triphenyllithium system, a bis(titanocenes) / alkylaluminum / silicate system or a bis(titanocenes) / alkylaluminum / lithium-based metal compound system.
[0031] More preferably, the specific process of hydrogenation using the bis(triocene)titanium / alkylaluminum / lithium metal compound system is as follows:
[0032] Under an argon atmosphere, the copolymer solution and the diocene titanocene / alkyl aluminum / lithium metal compound composite catalyst were added in sequence to a dry high-temperature reactor. The gas in the reactor was replaced three times with hydrogen. The speed of the reactor was adjusted to 100-1000 rpm, the hydrogenation reaction pressure was 1.6-2.5 MPa, the temperature was increased to 30°C-100°C, and the reaction was carried out for 1-5 hours.
[0033] Further preferably, the catalyst bis(titanocenes) includes dichlorotitanocenes; the co-catalyst alkylaluminum is one or more of trimethylaluminum, tri-n-butylaluminum, triisobutylaluminum, triethylaluminum, diethylaluminum monochloride, ethylaluminum dichloride, and diisobutylaluminum hydride; and the lithium-based metal compound is one or more of lithium methoxide, lithium ethoxide, and phenyllithium.
[0034] More preferably, the mass ratio of the copolymer to the titanocene in the copolymer solution is (1-6000):1; the molar ratio of the titanocene to the alkyl aluminum compound is 1:(1-8), and the molar ratio of the titanocene to the lithium metal compound is 1:(1-10).
[0035] The third object of the present invention is to provide a hydrogenated conjugated diene and bio-based terpene multi-random copolymer for use in the fields of solar photovoltaic films, automotive parts, medical packaging materials, building materials, daily necessities and toys.
[0036] Compared with the prior art, the present invention has the following advantages:
[0037] (1) The present invention creatively proposes to first obtain a copolymer of conjugated diene and bio-based terpene through an iron-based coordination polymerization system, and then use a corresponding transition metal catalyst as a hydrogenation catalyst to hydrogenate the double bonds of the copolymer, and finally obtain a hydrogenated conjugated diene-bio-based terpene copolymer elastomer material, the molecular chain of which has a saturated single bond ratio of more than 90%, and has excellent weather resistance, mechanical strength and ductility, and has the properties of POE, and has a certain substitution for POE. At the same time, the hydrogenated material has a longer side chain, so it has better impact resistance than POE. Due to various factors such as the technical barriers of catalysts, the supply of raw materials α-olefins and the lack of polymerization processes, China has not yet completely gotten rid of its dependence on POE products. The present invention creatively proposes a method for hydrogenating this new type of material, which can alleviate the dependence on foreign POE products and help break the monopoly of POE.
[0038] (2) The polymerization pathway proposed in the present invention has the characteristics of easy availability of raw materials, simple operation, and environmentally friendly components. The system has high catalytic activity and a monomer conversion rate of more than 90%. At the same time, the hydrogenation process is optimized to further reduce the hydrogenation cost, and the overall hydrogenation degree of the polymer reaches more than 95%. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 The binary random copolymer obtained in step (1) of Example 1 1 H NMR spectrum;
[0040] Figure 2 The hydrogenation product obtained in step (2) of Example 1 1 H NMR spectrum;
[0041] Figure 3 This is the GPC spectrum of the hydrogenation product obtained in step (2) of Example 1;
[0042] Figure 4 This is the DSC spectrum of the hydrogenation product obtained in step (2) of Example 1. DETAILED DESCRIPTION
[0043] As used herein, the terms "comprises," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, step, method, article, or apparatus comprising the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, step, method, article, or apparatus.
[0044] When equivalent, concentration or other value or parameter is represented with scope, preferred range or a series of upper preferred value and lower preferred value limit scope in the present invention, this should be understood as specifically disclosing all scopes formed by any pairing of any upper range limit or preferred value and any lower range limit or preferred value, regardless of whether the scope is disclosed separately. For example, when disclosing scope "1 to 5", described scope should be interpreted as including scope "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5" etc. When numerical range is described in this article, unless otherwise stated, the scope is intended to include its end value and all integers and fractions within the scope. In the present application specification and claims, range limitation can be combined and / or interchanged, if these scopes are not otherwise stated, include all sub-ranges contained therein.
[0045] The indefinite articles "a" and "an" before the elements or components of the present invention have no limitation on the quantity requirements (i.e. the number of occurrences) of the elements or components. Therefore, "a" or "an" should be interpreted as including one or at least one, and the elements or components in the singular form also include the plural form, unless the quantity obviously refers to the singular form only.
[0046] The "one embodiment" or "embodiment" of the present invention refers to a specific feature, structure or characteristic that can be included in at least one implementation of the present invention. The "in one embodiment" that appears in different places in this specification does not refer to the same embodiment, nor is it a separate or selective embodiment that is mutually exclusive with other embodiments.
[0047] The endpoints and any values of the ranges disclosed in the invention are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in this article.
[0048] The present invention provides a hydrogenated conjugated diene and bio-based terpene multi-component random copolymer, wherein the copolymer is formed by copolymerizing and hydrogenating at least one of the conjugated diene monomers and at least one of the bio-based terpene monomers, wherein the general formula of the conjugated diene monomer is C n H 2n-2 , n≥4, the general formula of bio-based terpene monomer is (C5H8) n , n≥2, the molar content of conjugated diene polymerization units is 10% to 90%, the molar content of bio-based terpene polymerization units is 10% to 90%, and the degree of hydrogenation is 90% to 99.9%.
[0049] Preferably, the conjugated diene monomer includes 1,3-butadiene, isoprene, 1,5-hexadiene or 1,7-octadiene, and the bio-based terpene monomer includes limonene, α-pinene, β-pinene, α-myrcene, β-myrcene, α-farnesene or β-farnesene.
[0050] Further preferably, the conjugated diene monomer is isoprene or 1,3-butadiene, and the bio-based terpene monomer is β-myrcene or β-farnesene.
[0051] Preferably, the copolymer has a number average molecular weight of 10,000 to 500,000 g / mol, a molecular weight distribution of 1.0 to 5.0, a glass transition temperature of -80°C to 20°C, a Shore A hardness of >40, a rebound elastic modulus of >20%, an elongation at break of >600%, a tear strength of >20 N / mm, and a volume resistivity of >0.6×10 18 Ω.cm, melting point 55℃~80℃, melt index 60~80g / 10min, heat deformation temperature>125℃, light transmittance at 380-1100nm>89%, water vapor transmittance<3.5%, low temperature notched impact strength (-30℃)>59kJ / m 2 , Izod notch impact strength>70kJ / m 2 .
[0052] Further preferably, the molecular weight distribution of the copolymer is 1.4 to 3.1, the degree of hydrogenation is 95% to 99%, the glass transition temperature range is -68°C to -25°C, the Shore A hardness is greater than 52, the rebound elastic modulus is greater than 23%, the elongation at break is greater than 650%, the tear strength is greater than 27N / mm, and the volume resistivity is greater than 0.76×10 18 Ω.cm, melting point 62℃~69℃, melt index 66~76g / 10min, heat deformation temperature>132℃, light transmittance at 380-1100nm>92%, water vapor transmittance<2.8%, low temperature notched impact strength (-30℃)>62kJ / m 2 , Izod notch impact strength>76kJ / m 2 .
[0053] The present invention also provides a method for preparing a hydrogenated conjugated diene and bio-based terpene multi-component random copolymer, the method being carried out according to the following steps:
[0054] (1) preparing a multi-component random copolymer by copolymerizing a conjugated diene monomer and a bio-based terpene monomer;
[0055] (2) The multi-component random copolymer is dissolved in a solvent to obtain a copolymer solution, and then hydrogenated by a Ziegler-Natta hydrogenation reaction system or a metallocene hydrogenation reaction system to obtain a hydrogenated conjugated diene and bio-based terpene multi-component random copolymer.
[0056] Preferably, the preparation of the multi-component random copolymer in step (1) is carried out by anionic polymerization, cationic polymerization, free radical polymerization or coordination polymerization. More preferably, it is coordination polymerization, anionic polymerization or free radical polymerization. More preferably, it is coordination polymerization or anionic polymerization.
[0057] Preferably, the coordination polymerization method includes iron coordination polymerization, Zignata type catalyst system polymerization, β-diaminosulfonate as a ligand cationic lutetium coordination complex polymerization, rare earth lanthanide catalytic polymerization system polymerization, [OSSO] type titanium complex polymerization, half sandwich scandium complex polymerization, cobalt catalyst system polymerization. More preferably, it is iron coordination polymerization, β-diaminosulfonate as a ligand cationic lutetium coordination complex polymerization, rare earth lanthanide catalytic polymerization system polymerization, [OSSO] type titanium complex polymerization, cobalt catalyst system polymerization. More preferably, it is iron coordination polymerization, β-diaminosulfonate as a ligand cationic lutetium coordination complex polymerization, rare earth lanthanide catalytic polymerization system polymerization. Most preferably, it is iron coordination polymerization.
[0058] When the preparation of the multi-component random copolymer adopts the iron coordination polymerization method, the specific steps are: under anhydrous and oxygen-free conditions, an iron catalyst, a co-catalyst, a conjugated diene monomer, a bio-based terpene monomer and a solvent are added to a reactor, and the polymerization reaction is stirred at -30°C to 100°C for 10min to 120min. After the reaction, a quencher and an antioxidant are added after washing, and vacuum drying is performed to constant weight to obtain a multi-component random copolymer of conjugated diene and bio-based terpene.
[0059] More preferably, the reaction temperature is -20°C to 30°C, and the reaction time is 30 min.
[0060] When the iron coordination polymerization method is adopted, the iron catalyst is any one of the following structural formulas:
[0061]
[0062] Further preferably, the solvent is one or more of cyclohexane, n-hexane, petroleum ether, toluene, and xylene, and the ratio of the solvent to the total volume of the comonomer is (1-50):1, more preferably (3-10):1; the molar ratio of the total molar amount of the comonomer to the iron element in the iron catalyst is (100-50000):1, more preferably 200-20000:1.
[0063] Further preferably, the co-catalyst is a single component or a two-component. When the co-catalyst is a single component, the co-catalyst is selected from one or more of methylaluminoxane (MAO), dried methylaluminoxane (DMAO), and modified methylaluminoxane (MMAO). The molar ratio of the aluminum element in the co-catalyst to the iron element in the iron catalyst is (100-1500):1, more preferably 500:1; when the co-catalyst is a two-component, component A is selected from one or more of trimethylaluminum, tri-n-butylaluminum, triisobutylaluminum, triethylaluminum, diethylaluminum monochloride, ethylaluminum dichloride, diisobutylaluminum hydride, and sesquiethylaluminum chloride. , component B is one or more of methylaluminoxane (MAO), dried methylaluminoxane (DMAO), modified methylaluminoxane (MMAO), N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, 4-isopropyl-4'-methyldiphenyl iodide tetrakis(pentafluorophenyl)borate, triphenylphosphine oxide, tris(pentafluorophenyl)phosphine, and triphenylphosphine, the molar ratio of aluminum element in component A to iron element in the iron catalyst is (1-100):1, more preferably 40:1, and the molar ratio of aluminum, boron or phosphine element in component B to iron element in the iron catalyst is (1-20):1, more preferably 1:1.
[0064] When the multi-component random copolymer is prepared by anionic polymerization, the specific steps are: under anhydrous and oxygen-free conditions, an organic alkali metal is used as an initiator to initiate copolymerization of a conjugated diene monomer and a bio-based terpene monomer, and after reacting at a certain temperature for a certain time, ethanol is added to quench the reaction and obtain a polymerization product;
[0065] Alternatively, under anhydrous and oxygen-free conditions, an organic alkali metal is used as an initiator and an organic aluminum compound is used as a co-catalyst to initiate the copolymerization of a conjugated diene monomer and a bio-based terpene monomer. After reacting at a certain temperature for a certain time, ethanol is added to quench the reaction and obtain a polymerization product.
[0066] Preferably, the organic alkali metal is one or more of n-butyllithium, sec-butyllithium, tert-butyllithium, lithium tert-butoxide, methyllithium, ethyllithium, n-propyllithium, isopropyllithium, phenyllithium, benzyllithium, and naphthalenelithium; more preferably, it is one or more of n-butyllithium, sec-butyllithium, tert-butyllithium, and n-propyllithium.
[0067] Preferably, the reaction temperature is -50°C to 70°C, and the reaction time is 10 min to 360 min; more preferably, the reaction temperature is 30°C, and the reaction time is 30 min.
[0068] Preferably, the solvent is one or more of THF, toluene, ethylbenzene, xylene, n-hexane, cyclohexane, dichloromethane, chloroform, ethyl ether, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, and methyl tert-butyl ether; more preferably, it is one or more of THF, toluene, ethylbenzene, n-hexane, cyclohexane, ethylene glycol dimethyl ether, and methyl tert-butyl ether.
[0069] Preferably, the organoaluminum compound can be abbreviated as AB, wherein A represents one or more of trimethylaluminum, triethylaluminum, triisobutylaluminum, diethylaluminum monochloride, ethylaluminum dichloride or sesquiethylaluminum chloride, and B represents one or more of 2,6-di-tert-butyl-p-cresol, table 2,6-di-tert-butylphenol, 2-tert-butylphenol or 2,6-di-tert-butyl-4-ethylphenol, and the molar ratio of A to B is (0.1 to 2):1.
[0070] Preferably, the ratio of the total volume of the solvent to the comonomer is (1-50):1, more preferably 3:1; the molar ratio of the total molar amount of the comonomer to the lithium element in the initiator is (100-50000):1, more preferably 2000:1; the molar ratio of the total molar amount of the comonomer to the aluminum element in the co-catalyst is (13-6250):1, more preferably 250:1.
[0071] When the preparation of the multi-component random copolymer adopts a free radical polymerization method, examples thereof include: hydrogen peroxide polymerization, emulsion polymerization, nitroxide free radical polymerization (NMP), reversible addition chain transfer polymerization (RAFT), etc. Among these methods, nitroxide free radical polymerization (NMP) and reversible addition chain transfer free radical polymerization are preferred; reversible addition chain transfer free radical polymerization is most preferred, and the initiator is one or more of azobisisobutyronitrile, benzoyl peroxide, azobisisoheptanenitrile, azobishydroxyvaleric acid, dimethyl azobisisobutyrate, azobisisobutyramidine hydrochloride, azobisisobutylimidazoline hydrochloride, and azoisobutylcyanoformamide.
[0072] When the multi-component random copolymer is prepared by cationic polymerization, examples thereof include: cationic polymerization of β-myrcene using a dispersible Lewis acid surfactant combination catalyst (LASC) prepared from ytterbium chloride and sodium alkylbenzene sulfonate surfactant; trifluoromethanesulfonate initiation system, boron trifluoride ether initiation system, etc. Among these methods, the LASC polymerization method is preferred.
[0073] Preferably, the polymerization reaction can be quenched by adding a protic compound such as methanol, a methanol solution of acetic acid or a methanol solution of hydrochloric acid; an aqueous solution of acetic acid or hydrochloric acid to the reaction solution.
[0074] Preferably, the concentration of the copolymer solution in step (2) is 10 wt %.
[0075] Preferably, the solvent of the copolymer solution in step (2) is one or more of toluene, xylene, n-hexane and cyclohexane.
[0076] Preferably, in step (2), when a Ziegler-Natta hydrogenation reaction system is used, the specific process of hydrogenation is:
[0077] In an argon atmosphere, the copolymer solution, catalyst and co-catalyst are added to a dry high-temperature reactor in sequence, and the gas in the reactor is replaced three times with hydrogen. The speed of the reactor is adjusted to 100-1000rpm, the hydrogenation reaction pressure is 1-5MPa, the temperature is raised to 95℃-120℃, and the reaction is carried out for 1-5h. After the reaction is completed, the system is cooled to room temperature, anhydrous ethanol is poured, and the hydrogenated elastomer is separated in the form of a precipitate. The precipitate is placed in a vacuum oven and dried at room temperature to a constant weight to obtain the final hydrogenated conjugated diene and bio-based terpene multi-random copolymer.
[0078] Further preferably, the catalyst is one or more of nickel sulfate, nickel chloride, nickel nitrate or nickel cyclohexaneate, and nickel cyclohexaneate is most preferred; the co-catalyst is an organic metal compound of a metal from Group IA to Group IIIA, and more preferably is one or more of trimethylaluminum, tri-n-butylaluminum, triisobutylaluminum, triethylaluminum, diethylaluminum monochloride, ethylaluminum dichloride, and diisobutylaluminum hydride, and most preferably is triisobutylaluminum.
[0079] Further preferably, the mass ratio of the copolymer and the catalyst in the copolymer solution is (1-500):1, more preferably 350:1; the molar ratio of the catalyst and the co-catalyst is 1:(1-20), more preferably 1:5; the hydrogenation reaction temperature is preferably 100°C; the hydrogenation reaction pressure is preferably 3MPa; the rotation speed of the hydrogenation reactor is preferably 600rpm; and the hydrogenation reaction time is preferably 2.5h.
[0080] Preferably, the metallocene hydrogenation reaction system in step (2) comprises a bis(titanocenes) / lithium hydride / aromatic ester system, a bis(titanocenes) or mono(titanocenes) / triphenyllithium system, a bis(titanocenes) / alkylaluminum / silicate system or a bis(titanocenes) / alkylaluminum / lithium-based metal compound system.
[0081] More preferably, the specific process of hydrogenation using the bis(triocene)titanium / alkylaluminum / lithium metal compound system is as follows:
[0082] In an argon atmosphere, the copolymer solution and the di-titaniumocene / alkyl aluminum / lithium metal compound composite catalyst are sequentially added to a dry high-temperature reactor, and the gas in the reactor is replaced three times with hydrogen. The speed of the reactor is adjusted to 100-1000rpm, the hydrogenation reaction pressure is 1.6-2.5MPa, the temperature is raised to 30℃-100℃, and the reaction is carried out for 1-5h. After the reaction is completed, the system is cooled to room temperature, anhydrous ethanol is poured, and the hydrogenated elastomer is separated in the form of a precipitate. The precipitate is placed in a vacuum oven and dried at room temperature to a constant weight to obtain the final hydrogenated conjugated diene and bio-based terpene multi-random copolymer.
[0083] Further preferably, the catalyst bis-titanocenes include titanocene dichloride; the co-catalyst alkyl aluminum is one or more of trimethyl aluminum, tri-n-butyl aluminum, triisobutyl aluminum, triethyl aluminum, diethyl aluminum monochloride, ethyl aluminum dichloride, and diisobutyl aluminum hydride, more preferably triisobutyl aluminum; the lithium-based metal compound is one or more of lithium methoxide, lithium ethoxide, and phenyl lithium, more preferably lithium ethoxide.
[0084] Further preferably, the mass ratio of the copolymer and the bis(trifluoromethyl)titanium in the copolymer solution is (1-6000):1, more preferably 4000:1; the molar ratio of the bis(trifluoromethyl)titanium and the alkylaluminum compound is 1:(1-8), more preferably 1:4.5; the molar ratio of the bis(trifluoromethyl)titanium and the lithium metal compound is 1:(1-10), more preferably 1:6; the hydrogenation reaction temperature is preferably 50°C; the hydrogenation reaction pressure is preferably 1.7 MPa; the rotation speed of the hydrogenation reactor is preferably 600 rpm; and the hydrogenation reaction time is preferably 1.5 h.
[0085] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0086] The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, methods and instruments used are conventional materials, reagents, methods and instruments in the art unless otherwise specified, and can be obtained through commercial channels by those skilled in the art.
[0087] The terms "comprising," "including," "having," "containing," or any other variations thereof, as used in the following examples, are intended to cover a non-exclusive inclusion. For example, a composition, step, method, article, or apparatus comprising the listed elements is not necessarily limited to only those elements, but may include other elements not expressly listed or inherent to such composition, step, method, article, or apparatus.
[0088] In the following examples, when equivalent, concentration or other values or parameters are represented by range, preferred range or a series of upper preferred values and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any upper range limit or preferred value and any lower range limit or preferred value, regardless of whether the scope is disclosed separately. For example, when disclosing scope "1 to 5", described scope should be interpreted as including scope "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5" etc. When numerical range is described in this article, unless otherwise stated, the scope is intended to include its end value and all integers and fractions within the scope. In the present application specification and claims, range limitation can be combined and / or interchanged, if these scopes are not otherwise stated, include all sub-ranges contained therein.
[0089] In the following embodiments, the indefinite articles "a" and "an" before the elements or components have no restrictions on the quantity requirements (i.e., the number of occurrences) of the elements or components. Therefore, "a" or "an" should be interpreted as including one or at least one, and the elements or components in the singular form also include the plural form, unless the number obviously refers to the singular form only.
[0090] The "one embodiment" or "embodiment" described in the following embodiments refers to a specific feature, structure or characteristic that can be included in at least one implementation of the present invention. The "in one embodiment" that appears in different places in this specification does not refer to the same embodiment, nor is it a separate or selective embodiment that is mutually exclusive with other embodiments.
[0091] The endpoints and any values of the ranges disclosed in the following examples are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be considered as specifically disclosed in this article.
[0092] The mechanical properties test standard in the following embodiments is GB / T 589-2009;
[0093] The light transmittance test standard is: ASTM D1003-2021;
[0094] Melt index test standard: ASTM D 1238;
[0095] The water vapor transmission rate test standard is: GB / T 1037-2021;
[0096] Low temperature notched impact strength test standard: ISO179-1:2010;
[0097] The cantilever beam notched impact strength test standard is: refer to ISO180-2019;
[0098] Thermal deformation temperature detection standard: refer to GB / T1634-2019;
[0099] Ohmmeter: Keithley; Model 6517B, 1000v, 10min.
[0100] Example 1: The steps of preparing a hydrogenated conjugated diene-bioterpene multi-component random copolymer of this example are as follows:
[0101] (1) Polymerization: In an argon atmosphere, anhydrous toluene (24 mL), isoprene (1.4 mL, 14.0 mmol, 1400 equiv.), β-myrcene (1 mL, 6 mmol, 600 equiv.), MAO (5.0 mmol, 500 equiv.), and iron catalyst 1 (1.0 ml, 10 μmol, 1 equiv.) were added to a 100 mL Schlenk tube in sequence, and the polymerization was carried out at -20°C for 30 min, and then the reaction was terminated with 25 mL of a mixed solution of methanol and hydrochloric acid (MeOH / HCl volume ratio = 50 / 1) and 1 mL of an antioxidant. After the clear liquid was discarded, the polymer was washed three times with ethanol, and the obtained polymer was placed at 40°C and vacuum dried to constant weight to obtain an elastomeric polymer.
[0102] (2) Hydrogenation: A xylene mother liquor (10 wt%) of the copolymer was prepared in a 100 mL Schlenk tube. 50.0 mL of the xylene mother liquor (10 wt%) of the copolymer, catalyst nickel cyclohexaneate (14.3 mg, 35.6 μmol, 1 equiv.), and co-catalyst triethylaluminum (0.18 mL, 178 μmol, 5 equiv.) were added to the Schlenk tube in argon atmosphere, and stirred at 600 rpm for 20 min. H2 was used to replace the gas three times. After the stamping, the pressure in the reactor was 3 MPa. Stirring was turned on, the hydrogenation temperature was 100 ° C, the hydrogenation time was 2.5 h, and the speed was 600 rpm. After the reaction was completed, the hydrogenation kettle was cooled to room temperature, and after the pressure was released, it was left to stand for 30.0 min and then opened. After post-treatment, a white elastomer was obtained.
[0103] Example 2: This example is different from Example 1 in that the amount of MAO added in step (1) is changed to (50.0 mmol, 5000 equiv.), the amount of iron catalyst 1 added is changed to (10.0 ml, 100 μmol, 10 equiv.), and the other steps and parameters are the same as in Example 1.
[0104] Example 3: This example differs from Example 1 in that the reaction is carried out in a 500 mL Schlenk tube, the amount of anhydrous toluene added in step (1) is (240 mL), the amount of isoprene added is (14 mL, 140.0 mmol, 14000 equiv.), the amount of β-myrcene added is (10 mL, 60 mmol, 6000 equiv.), and the other steps and parameters are the same as in Example 1.
[0105] Example 4: This example is different from Example 1 in that the amount of anhydrous toluene added in step (1) is (17 mL), the amount of β-myrcene added is (0.26 mL, 1.6 mmol, 156 equiv.), and the other steps and parameters are the same as in Example 1.
[0106] Example 5: This example differs from Example 1 in that in step (1), the amount of anhydrous toluene added is (25 mL), the amount of isoprene added is (0.16 mL, 1.6 mmol, 156 equiv.), the amount of β-myrcene added is (2.3 mL, 14 mmol, 1400 equiv.), and the other steps and parameters are the same as in Example 1.
[0107] Example 6: This example differs from Example 1 in that the reaction is carried out in a 50 mL Schlenk tube, the amount of anhydrous toluene added in step (1) is (7.2 mL), and the other steps and parameters are the same as in Example 1.
[0108] Example 7: This example differs from Example 1 in that the iron catalyst in step (1) is replaced with iron catalyst 7 (1.0 ml, 10 μmol, 1 equiv.), and the other steps and parameters are the same as those in Example 1.
[0109] Example 8: This example differs from Example 1 in that the amount of anhydrous toluene added in step (1) is (27 ml), the bio-based terpene in the comonomer is replaced by β-myrcene with β-farnesene (1.7 ml, 6 mmol, 600 equiv.), and the other steps and parameters are the same as in Example 1.
[0110] Example 9: This example differs from Example 1 in that the amount of anhydrous toluene added in step (1) is (21 ml), the conjugated diene in the comonomer is replaced by 1,3-butadiene (1.14 mL, 14.0 mmol, 1400 equiv.), and the other steps and parameters are the same as in Example 1.
[0111] Example 10: This example differs from Example 1 in that the amount of anhydrous toluene added in step (1) is (28 ml), the conjugated diene in the comonomer is replaced by isoprene with 1,3-butadiene (1.14 ml, 14.0 mmol, 1400 equiv.), the bio-based terpene is replaced by β-myrcene with β-farnesene (1.7 ml, 6 mmol, 600 equiv.), and the other steps and parameters are the same as in Example 1.
[0112] Example 11: This example differs from Example 1 in that anhydrous toluene (28 mL), isoprene (1.4 mL, 14.0 mmol, 1400 equiv.), β-myrcene (0.52 mL, 3 mmol, 300 equiv.) and β-farnesene (0.84 mL, 3 mmol, 300 equiv.) were used, and the other steps and parameters were the same as those in Example 1.
[0113] Example 12: This example differs from Example 1 in that anhydrous toluene (25 mL) is used, the polymerization monomer isoprene is replaced with 1,3-butadiene, and the amount of 1,3-butadiene added is (1.14 mL, 14.0 mmol, 1400 equiv.), and the other steps and parameters are the same as those in Example 1.
[0114] Example 13: This example is different from Example 1 in that: anhydrous toluene (25 mL), isoprene (1.08 mL, 10.8 mmol, 1080 equiv.), 1,3-butadiene (0.88 mL, 10.8 mmol, 1080 equiv.), β-myrcene (0.2 mL, 1.2 mmol, 120 equiv.), β-farnesene (0.34 mL, 1.2 mmol, 120 equiv.), and the other steps and parameters are the same as in Example 1.
[0115] Example 14: This example is different from Example 1 in that the copolymerization method in step (1) uses anionic polymerization, and the specific steps are:
[0116] (1) Polymerization: Under argon atmosphere, anhydrous toluene (7.2 mL), i-BuAl(BHT) and 1.9 (5mL, 1.6mmol, 8equiv.) aluminum reagent, initiator sec-butyl lithium (0.15mL, 0.2mmol, 1equiv.) and isoprene (1.4mL, 14.0mmol, 1400equiv.), β-myrcene (1mL, 6mmol, 600equiv.), polymerize at 30°C for 30min, and then terminate the reaction with 25mL of a mixed solution of methanol and hydrochloric acid (MeOH / HCl volume ratio = 50 / 1) and 1mL of an antioxidant. After pouring off the clear liquid, the polymer is washed three times with ethanol, and the obtained polymer is placed at 40°C and vacuum dried to constant weight to obtain an elastomeric polymer. Other steps and parameters are the same as those in Example 1.
[0117] Example 15: This example is different from Example 1 in that the hydrogenation reaction system in step (2) is replaced with a bis(pentacyclopentadienyl)titanium / alkylaluminum / lithium metal compound system. The specific steps are:
[0118] (2) Hydrogenation: A xylene mother solution (10 wt%) of the copolymer was prepared in a 100 mL Schlenk tube. The reactor was dried and heated to 70°C. 50.0 mL of the xylene mother solution (10 wt%) of the copolymer and a catalyst, dichlorotantalum (0.31 mg, 1.25 μmol, 1 equiv.), and a co-catalyst, triisobutylaluminum (0.16 mL, 162 μmol, 4.5 equiv.), and lithium ethoxide (0.21 mL, 7.5 μmol, 6 equiv.) were added successively under an argon atmosphere. The mixture was stirred at 600 rpm for 20 min. H2 was used to replace the gas three times. After the press, the pressure in the reactor was 1.7 MPa. Stirring was started. The hydrogenation temperature was 50°C, the hydrogenation time was 1.5 h, and the rotation speed was 600 rpm. After the reaction, the hydrogenation reactor was cooled to room temperature. After the pressure was released, the reactor was left to stand for 30.0 min and then opened for post-treatment to obtain a white elastomer. The other steps and parameters were the same as those in Example 1.
[0119] Table 1 Test data of hydrogenated conjugated diene and bio-based terpene multi-random copolymer elastomers of Examples 1-8
[0120]
[0121] Table 2 Test data of hydrogenated conjugated diene and bio-based terpene multi-random copolymer elastomers of Examples 9-15
[0122]
[0123]
[0124] The above are only preferred specific embodiments of the present invention, which are all different implementations based on the overall concept of the present invention, and the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A hydrogenated conjugated diene and bio-based terpene multi-random copolymer, characterized in that: The copolymer is formed by copolymerizing and hydrogenating at least one of the conjugated diene monomers and at least one of the bio-based terpene monomers, wherein the conjugated diene monomer has a general formula of C n H 2n-2 , n≥4, the general formula of bio-based terpene monomer is (C5H8) n , n≥2, the molar content of conjugated diene-based polymerization units is 10% to 90%, the molar content of bio-based terpene-based polymerization units is 10% to 90%, and the degree of hydrogenation is 90% to 99.9%.
2. The copolymer according to claim 1, characterized in that The conjugated diene monomers include 1,3-butadiene, isoprene, 1,5-hexadiene, and 1,7-octadiene, and the bio-based terpene monomers include limonene, α-pinene, β-pinene, α-myrcene, β-myrcene, α-farnesene, and β-farnesene.
3. The copolymer according to claim 2, characterized in that The conjugated diene monomer is isoprene or 1,3-butadiene, and the bio-based terpene monomer is β-myrcene or β-farnesene.
4. The copolymer according to claim 1, characterized in that The number average molecular weight of the copolymer is 10,000 to 500,000 g / mol, the molecular weight distribution is 1.0 to 5.0, the glass transition temperature is -80°C to 20°C, the Shore A hardness is greater than 40, the rebound elastic modulus is greater than 20%, the elongation at break is greater than 600%, the tear strength is greater than 20N / mm, and the volume resistivity is greater than 0.6×10 18 Ω.cm, melting point 55℃~80℃, melt index 60~80g / 10min, heat deformation temperature>125℃, light transmittance at 380-1100nm>89%, water vapor transmittance<3.5%, low temperature notched impact strength (-30℃)>59kJ / m 2 , Izod notch impact strength>70kJ / m 2 .
5. The copolymer according to claim 4, characterized in that The molecular weight distribution is 1.4 to 3.1, the degree of hydrogenation is 95% to 99%, the glass transition temperature range is -68℃ to -25℃, the Shore hardness A>52, the rebound elastic modulus>23%, the elongation at break>650%, the tear strength>27N / mm, and the volume resistivity>0.76×10 18 Ω.cm, melting point 62℃~69℃, melt index 66~76g / 10min, heat deformation temperature>132℃, light transmittance at 380-1100nm>92%, water vapor transmittance<2.8%, low temperature notched impact strength (-30℃)>62kJ / m 2 , Izod notch impact strength>76kJ / m 2 .
6. The method for preparing the copolymer according to any one of claims 1 to 5, characterized in that: The method: (1) preparing a multi-component random copolymer by copolymerizing a conjugated diene monomer and a bio-based terpene monomer; (2) The multi-component random copolymer is dissolved in a solvent to obtain a copolymer solution, and then hydrogenated by a Ziegler-Natta hydrogenation reaction system or a metallocene hydrogenation reaction system to obtain a hydrogenated conjugated diene and bio-based terpene multi-component random copolymer.
7. The method according to claim 6, characterized in that The copolymerization in step (1) adopts anionic polymerization, cationic polymerization, free radical polymerization or coordination polymerization.
8. The method according to claim 7, characterized in that The specific process of anionic polymerization is as follows: The copolymerization is initiated under anhydrous and oxygen-free conditions with an organic alkali metal as an initiator and / or an organic aluminum compound as a co-catalyst.
9. The method according to claim 8, characterized in that The organic alkali metal is one or more of n-butyllithium, sec-butyllithium, tert-butyllithium, lithium tert-butoxide, methyllithium, ethyllithium, n-propyllithium, isopropyllithium, phenyllithium, benzyllithium, and naphthalenelithium; the organic aluminum compound is abbreviated as AB, wherein A represents one or more of trimethylaluminum, triethylaluminum, triisobutylaluminum, diethylaluminum monochloride, ethylaluminum dichloride, or sesquiethylaluminum chloride; B represents one or more of 2,6-di-tert-butyl-p-cresol, table 2,6-di-tert-butylphenol, 2-tert-butylphenol, or 2,6-di-tert-butyl-4-ethylphenol; the reaction temperature is -50°C to 70°C; and the reaction time is 10 min to 360 min.
10. The method according to claim 9, characterized in that The reaction temperature was 30°C and the reaction time was 30 min.
11. The method according to claim 7, characterized in that Coordination polymerization methods include iron coordination polymerization, Zignata-type catalytic system polymerization, cationic lutetium coordination complex polymerization with β-diaminosulfonate as ligand, rare earth lanthanum catalytic polymerization system polymerization, [OSSO] type titanium complex polymerization, half-sandwich scandium complex polymerization, and cobalt catalytic system polymerization.
12. The method according to claim 11, characterized in that The specific process of using iron coordination polymerization method: Under anhydrous and oxygen-free conditions, an iron catalyst, a co-catalyst, a conjugated diene monomer, a bio-based terpene monomer and a solvent are added into a reactor, and a polymerization reaction is carried out at -30 to 100° C. with stirring for 10 to 120 minutes.
13. The method according to claim 12, characterized in that The reaction temperature is -20°C to 30°C, and the reaction time is 30 minutes.
14. The method according to claim 12, characterized in that The iron catalyst is any one of the following structural formulas:
15. The method according to claim 6, characterized in that The concentration of the copolymer solution in step (2) is 10 wt %, and the solvent of the copolymer solution is one or more of toluene, xylene, n-hexane, and cyclohexane.
16. The method according to claim 6, characterized in that The Ziegler-Natta hydrogenation reaction process in step (2) is: Under an argon atmosphere, the copolymer solution, catalyst and co-catalyst are added in sequence to a dry high-temperature reactor, the gas in the reactor is replaced three times with hydrogen, and the reaction is carried out for 1 to 5 hours at a reactor speed of 100 to 1000 rpm, a hydrogenation reaction pressure of 1 to 5 MPa, and a temperature of 95°C to 120°C.
17. The method according to claim 16, characterized in that The catalyst is one or more of nickel sulfate, nickel chloride, nickel nitrate or nickel cyclohexaneate, the co-catalyst is an organic metal compound of metals from Group IA to Group IIIA, the mass ratio of the copolymer to the catalyst in the copolymer solution is (1-500):1, and the molar ratio of the catalyst to the co-catalyst is 1:(1-20).
18. The method according to claim 17, characterized in that The catalyst is nickel cyclohexaneate, and the co-catalyst is one or more of trimethylaluminum, tri-n-butylaluminum, triisobutylaluminum, triethylaluminum, diethylaluminum monochloride, ethylaluminum dichloride, and diisobutylaluminum hydride.
19. The method according to claim 6, characterized in that The metallocene hydrogenation reaction system in step (2) includes a bis(titaniacin) / lithium hydride / aromatic ester system, a bis(titaniacin) or mono(titaniacin) / triphenyllithium system, a bis(titaniacin) / alkylaluminum / silicate system or a bis(titaniacin) / alkylaluminum / lithium metal compound system.
20. The method according to claim 19, characterized in that The specific process of hydrogenation using the di-titanium / alkyl aluminum / lithium metal compound system is as follows: Under an argon atmosphere, the copolymer solution and the diocene titanocene / alkyl aluminum / lithium metal compound composite catalyst are added in sequence to a dry high-temperature reactor. The gas in the reactor is replaced three times with hydrogen. The reactor speed is 100-1000 rpm, the hydrogenation reaction pressure is 1.6-2.5 MPa, the temperature is increased to 30°C-100°C, and the reaction is carried out for 1-5 hours.
21. The method according to claim 20, characterized in that The bistitanocene includes dichlorobistitanocene, the alkyl aluminum is one or more of trimethyl aluminum, tri-n-butyl aluminum, triisobutyl aluminum, triethyl aluminum, diethyl aluminum monochloride, ethyl aluminum dichloride, and diisobutyl aluminum hydride, the lithium metal compound is one or more of lithium methoxide, lithium ethoxide, and phenyl lithium, the mass ratio of the copolymer and the bistitanocene in the copolymer solution is (1-6000):1, the molar ratio of the bistitanocene and the alkyl aluminum compound is 1:(1-8), and the molar ratio of the bistitanocene and the lithium metal compound is 1:(1-10).
22. The copolymer according to any one of claims 1 to 5 is used for producing solar photovoltaic films, automobile parts, medical packaging materials, building materials, daily products and toys.
Citation Information
Patent Citations
Ultrahigh melt index type styrene thermoplastic elastomer and preparation method thereof
CN114316164A
High-molecular-weight iron-based bio-based rubber, preparation method and application thereof, and rubber composition based on high-molecular-weight iron-based bio-based rubber
CN115073666A
Block copolymers containing a copolymer myrcene block
US20150284606A1