Crystalline radical polymerizable composition for electrical / electronic component, molded article for electrical / electronic component using said composition, and method for producing said molded article for electrical / electronic component
By using crystalline radical polymerizable compositions and inorganic filler materials in electrical and electronic parts sealing materials, the problems of low productivity and poor operability in the prior art are solved, and efficient use of electrical and electronic parts sealing and heat conducting materials are achieved. , suitable for electrical and electronic parts of complex shapes.
Patent Information
- Application Number
- CN202411034955.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2017-11-10
- Filing Date
- 2018-02-20
- Publication Date
- 2024-11-15
AI Technical Summary
In the prior art, the sealing molding method of liquid epoxy resin is low in productivity, and the specific usage method and curing agent of free radical polymeric resin are not recorded in detail, which makes it difficult to realize the characteristics of the molded product; the semiconductor sealing material has good fluidity at room temperature but The operability is poor, and the fluidity of the heat conducting material is reduced, and its usability is limited.
An electrical and electronic parts sealing material containing crystalline radical polymerizable compositions, inorganic fillers, silane coupling agents and radical polymerization initiators was developed, and the fluidity of the material was ensured by injection molding or transfer molding. and operability.
It realizes high productivity sealing of electrical and electronic parts, ensures excellent fluidity and operability, and improves heat conductivity, and is suitable for electrical and electronic parts sealing bodies of complex shapes.
Smart Images

Figure BDA0004970824240000351 
Figure BDA0004970824240000421
Abstract
Description
[0001] The present application is a divisional application of a patent application with application number "201880015561.5", application date "February 20, 2018", and invention name "Crystallized free radical polymerizable composition for electrical and electronic parts, electrical and electronic parts molded body using the composition, and method for manufacturing the electrical and electronic parts molded body". Technical Field
[0002] The present invention relates to a crystalline radical polymerizable composition for sealing electric and electronic parts, a sealed electric and electronic part body sealed with the composition, a granular material containing the crystalline radical polymerizable composition for sealing electric and electronic parts, and a method for producing a sealed electric and electronic part body.
[0003] The present invention also relates to a crystalline radically polymerizable composition for an electric or electronic component, an electric or electronic component molded body molded from the composition, a granular material containing the crystalline radically polymerizable composition for an electric or electronic component, and a method for producing the electric or electronic component molded body. Background Art
[0004] Electrical and electronic parts used in automobiles and electrical products are protected by metal or resin materials in order to avoid being affected by external factors such as dust, moisture, and impact. The sealing of electrical and electronic parts using metal is highly reliable, but it is expensive, so it is gradually being replaced by sealing materials made of cheap and productive resin materials. In addition, by changing the sealing of electrical and electronic parts using metal to resin sealing materials, electrical insulation is achieved, so the sealed electrical and electronic parts can be reduced in size, increasing the design freedom of the automobiles and electrical products on which they are mounted. In addition, electrical and electronic parts are also used under harsh conditions of high temperature and high humidity environments, so when using resin materials, most of them use thermosetting resins with excellent heat resistance.
[0005] Recently, liquid epoxy resins are used, which have good adhesion to resin substrates or metals and are excellent in mechanical strength and fluidity.
[0006] With the electronic control of automobiles, as well as the popularity of mobile devices and information appliances, the use of semiconductors has also increased significantly, and the importance of semiconductor sealing, one of the sealed electrical and electronic parts, is also increasing. The semiconductor sealing material used for semiconductor sealing is mostly ingot sheet epoxy molding compound (EMC). EMC is used in the transfer molding method with high productivity. Due to its excellent physical properties such as tightness and linear expansion coefficient, it ensures high reliability, but it requires frozen storage and post-curing steps, so the method of use needs to be simplified.
[0007] Therefore, in the past, epoxy resin compositions for sealing, electronic devices, automobiles, and methods for manufacturing electronic devices are known (e.g., Patent Document 1). In addition, methods for manufacturing semiconductor devices and acrylic resin compositions for semiconductor sealing used therein are known (e.g., Patent Document 2).
[0008] In addition, electrical and electronic parts used in automobiles and electrical products continue to deteriorate due to the heat generated by the electrical and electronic parts. Therefore, heat is effectively dispersed through metal wiring and metal casings such as aluminum. Metal casings also exceed the specifications, and there are also requirements for productivity, shape freedom, and insulation, so they are gradually being replaced by resins. In addition, when using resin materials, in order to impart thermal conductivity, a large amount of inorganic filler materials need to be added, so thermosetting resins with low resin viscosity and excellent heat resistance are used.
[0009] Therefore, a thermally conductive resin composition has been known in the past (for example, Patent Document 3). Also, an unsaturated polyester resin composition and a sealed motor have been known (for example, Patent Document 4).
[0010] Prior art literature
[0011] Patent Literature
[0012] Patent Document 1: Japanese Patent Application Publication No. 2014-148586
[0013] Patent Document 2: Japanese Patent Application Publication No. 2015-2204
[0014] Patent Document 3: Japanese Patent No. 6041157
[0015] Patent Document 4: Japanese Patent No. 5727628 Summary of the invention
[0016] Problems to be solved by the invention
[0017] Sealing molding using liquid epoxy resin is produced by relatively low productivity methods such as compression molding and casting. Therefore, a highly productive production method has been desired.
[0018] In the above-mentioned patent document 1, the epoxy resin composition for sealing is molded by transfer molding. The epoxy resin composition used for transfer molding must return the resin composition stored in a frozen state to room temperature. If the epoxy resin composition is stored at room temperature, the fluidity is greatly reduced or it will not be completely cured during the molding time. Therefore, there is a problem of curing after several hours in order to obtain the necessary properties of the molded product.
[0019] In addition, in Patent Document 1, there are records of (meth)acrylate resin, unsaturated polyester resin, and diallyl phthalate resin as free radical polymerizable compounds as thermosetting resins, but there is no detailed record of specific usage methods, embodiments, etc. of these free radical polymerizable compounds. In addition, there is no record of free radical polymerization initiators in the curing agent, so even if (meth)acrylate resin, unsaturated polyester resin, and diallyl phthalate resin are used, the free radical polymerizable compound cannot be three-dimensionally crosslinked. Therefore, the curing agent recorded in Patent Document 1 is limited to those that can three-dimensionally crosslink epoxy resins. So in fact, Patent Document 1 is the content of the epoxy resin composition.
[0020] In the above-mentioned patent document 2, the acrylic resin composition for semiconductor sealing is liquid at room temperature. Since it is liquid at room temperature, the fluidity is very good, but since the acrylic resin composition is liquid at room temperature, it is sticky, and the workability and operability are poor, and it cannot be operated in the general molding machine used for the granular and ingot flake shapes of the room temperature solid. In addition, during casting, bubbles are easily left in the resin composition, so it is difficult to control the bubbles. In addition, the liquid resin composition, compared with the solid resin composition, when using inorganic filler, the filler is easy to settle, so there is a problem that it is not easy to obtain a uniform molded product.
[0021] Therefore, the present invention provides a crystalline radical polymerizable composition having excellent fluidity and good handleability.
[0022] In addition, in the above-mentioned Patent Document 3, a thermally conductive filler having concavoconvex shapes is used, so the resin composition has a high thermal conductivity. Generally speaking, a molding material having a high thermal conductivity is compounded with a large amount of thermally conductive filler, so that the fluidity is reduced, the moldability is poor, and the use is limited. In addition, the price of the material having insulating properties and high thermal conductivity is also high, and it lacks versatility, so the use is limited.
[0023] In the above-mentioned Patent Document 4, BMC (bulk molding compound) requires a dedicated injection molding machine, so a dedicated molding machine must be prepared. In addition, BMC lacks storage stability, so there is a problem of gelation in summer.
[0024] Therefore, the present invention provides a crystalline radically polymerizable composition having excellent thermal conductivity and good handleability.
[0025] Means for solving problems
[0026] The present inventors have conducted extensive studies on compositions containing at least a crystalline radically polymerizable compound from various viewpoints, and as a result, have found the crystalline radically polymerizable composition for sealing electric and electronic components of the present invention.
[0027] That is, the crystalline radically polymerizable composition for sealing electric and electronic components of the present invention is characterized by containing at least a crystalline radically polymerizable compound, an inorganic filler, a silane coupling agent, and a radical polymerization initiator.
[0028] In addition, in a preferred embodiment of the crystalline free radical polymerizable composition for sealing electrical and electronic parts of the present invention, it is characterized in that the above-mentioned crystalline free radical polymerizable compound contains one or more selected from unsaturated polyesters, epoxy (meth) acrylates, urethane (meth) acrylates, polyester (meth) acrylates, polyether (meth) acrylates, free radical polymerizable monomers, and free radical polymerizable polymers.
[0029] In a preferred embodiment of the crystalline radically polymerizable composition for sealing an electric or electronic component of the present invention, the crystalline radically polymerizable compound has a melting point in the range of 30 to 150°C.
[0030] In a preferred embodiment of the crystalline radical polymerizable composition for sealing an electric and electronic component of the present invention, the crystalline radical polymerizable composition is solid at 23°C.
[0031] In a preferred embodiment of the crystalline radical polymerizable composition for sealing electrical and electronic parts of the present invention, the crystalline radical polymerizable composition has a melt viscosity measured by a high-flow tester at a measurement temperature of 90° C., a die diameter of 0.5 mm and a length of 1.0 mm, and a pressure of 30 kgf / cm 2 7~1000Pa·s, or at a pressure of 1kgf / cm 2 When, it is 1~7Pa·s.
[0032] In a preferred embodiment of the crystalline radically polymerizable composition for sealing electric and electronic components of the present invention, the inorganic filler is contained in an amount of 50 to 95% by weight based on the total amount of the crystalline radically polymerizable composition.
[0033] In a preferred embodiment of the crystalline radically polymerizable composition for sealing an electric and electronic component of the present invention, the ratio of the crystalline radically polymerizable compound to the total amount of the radically polymerizable compound is 30 parts by weight or more.
[0034] In a preferred embodiment of the crystalline radically polymerizable composition for sealing an electric and electronic component of the present invention, the weight average molecular weight of the crystalline radically polymerizable compound is 100 to 100,000.
[0035] Furthermore, the sealed electric and electronic component of the present invention is characterized in that it is sealed with the crystalline radically polymerizable composition for sealing an electric and electronic component of the present invention.
[0036] Furthermore, the granular material of the present invention is characterized by comprising the crystalline radically polymerizable composition for sealing electric and electronic components of the present invention.
[0037] The method for producing a sealed electric and electronic component of the present invention is characterized by comprising the step of sealing an electric and electronic component by insert molding such as injection molding or transfer molding using the granular material comprising the crystalline radical polymerizable composition for sealing an electric and electronic component of the present invention.
[0038] The present inventors have conducted extensive studies on compositions containing at least a crystalline radically polymerizable compound from various viewpoints, and as a result, have found the crystalline radically polymerizable composition for electric and electronic components of the present invention.
[0039] That is, the crystalline radically polymerizable composition for electric and electronic components of the present invention is characterized by containing at least a crystalline radically polymerizable compound, an inorganic filler, a silane coupling agent, and a radical polymerization initiator.
[0040] In a preferred embodiment of the crystalline radically polymerizable composition for electric and electronic components of the present invention, the thermal conductivity of a molded product obtained by molding the crystalline radically polymerizable composition for electric and electronic components is 1.0 W / m·K or more.
[0041] In addition, in a preferred embodiment of the crystalline free radical polymerizable composition for electrical and electronic parts of the present invention, it is characterized in that the above-mentioned crystalline free radical polymerizable compound contains one or more selected from unsaturated polyesters, epoxy (meth) acrylates, urethane (meth) acrylates, polyester (meth) acrylates, polyether (meth) acrylates, free radical polymerizable monomers, and free radical polymerizable polymers.
[0042] In a preferred embodiment of the crystalline radically polymerizable composition for electric and electronic components of the present invention, the melting point of the crystalline radically polymerizable compound is within a range of 30 to 150°C.
[0043] In a preferred embodiment of the crystalline radical polymerizable composition for electric and electronic components of the present invention, the crystalline radical polymerizable composition is solid at 23°C.
[0044] In a preferred embodiment of the crystalline radically polymerizable composition for electric and electronic components of the present invention, the inorganic filler is contained in an amount of 40 to 95% by weight based on the total amount of the crystalline radically polymerizable composition.
[0045] In a preferred embodiment of the crystalline radically polymerizable composition for electric and electronic components of the present invention, the ratio of the crystalline radically polymerizable compound to the total amount of radically polymerizable compounds is 25 parts by weight or more.
[0046] In a preferred embodiment of the crystalline radically polymerizable composition for an electric or electronic component of the present invention, the weight average molecular weight of the crystalline radically polymerizable compound is 70 to 100,000.
[0047] Furthermore, the electric and electronic component molded product of the present invention is characterized in that it is molded using the crystalline radical polymerizable composition for an electric and electronic component of the present invention.
[0048] In a preferred embodiment of the electric and electronic component molded body of the present invention, the molded body has a thermal conductivity of 1.0 W / m·K or more.
[0049] Furthermore, the granular material of the present invention is characterized by comprising the crystalline radically polymerizable composition for electric and electronic components of the present invention.
[0050] In addition, the method for manufacturing an electrical and electronic component molded body of the present invention is characterized in that it has a molding step of molding the above-mentioned granular material containing the crystalline free radical polymerizable composition for electrical and electronic components of the present invention into an electrical and electronic component molded body by any method selected from the group consisting of injection molding, transfer molding, compression molding, and hot melt molding.
[0051] Effects of the Invention
[0052] According to the crystalline radical polymerizable composition for sealing electric and electronic parts of the present invention, the effect of excellent workability can be exerted. In addition, according to the method for manufacturing the sealed electric and electronic parts of the present invention, the crystalline radical polymerizable composition becomes a crystalline radical polymerizable composition with extremely low viscosity during heating and melting during injection molding and transfer molding, so that the necessary fluidity can be ensured when sealing the sealed electric and electronic parts.
[0053] Furthermore, according to the present invention, there can be provided a sealed electric and electronic component body sealed with the crystalline radically polymerizable composition for sealing an electric and electronic component.
[0054] Furthermore, the present invention can provide a method for producing a sealed electric and electronic component, comprising the step of sealing an electric and electronic component by insert molding a granular material, powder or ingot containing the crystalline radical polymerizable composition for sealing an electric and electronic component.
[0055] In addition, the crystalline radical polymerizable composition for electric and electronic parts of the present invention can exhibit excellent effects of thermal conductivity and handling. In addition, according to the method for manufacturing electric and electronic parts of the present invention, the radical polymerizable composition becomes a low-viscosity radical polymerizable composition during heating and melting during injection molding and transfer molding, so it can exhibit the advantageous effect of ensuring the necessary fluidity when molding electric and electronic parts. In addition, an electric and electronic part molded body molded from the crystalline radical polymerizable composition for electric and electronic parts of the present invention can be provided.
[0056] Furthermore, there can be provided a method for producing an electric and electronic component molded body using granules, powders, or ingots containing the crystalline radically polymerizable composition for an electric and electronic component of the present invention. DETAILED DESCRIPTION
[0057] First, one embodiment of the crystalline radically polymerizable composition for sealing electric and electronic components of the present invention will be described as follows.
[0058] The crystalline radical polymerizable composition for sealing electrical and electronic parts of the present invention is characterized in that it contains at least a crystalline radical polymerizable compound, an inorganic filler, a silane coupling agent, and a radical polymerization initiator. This is because by using a crystalline radical polymerizable composition, as shown in the examples described below, a polymerizable composition with excellent fluidity and excellent operability can be achieved. In addition, in this specification, the crystalline radical polymerizable composition for sealing electrical and electronic parts may be referred to as a crystalline radical polymerizable composition.
[0059] In addition, in a preferred embodiment of the crystalline free radical polymerizable composition for sealing electrical and electronic parts of the present invention, it is characterized in that the above-mentioned crystalline free radical polymerizable compound contains one or more selected from unsaturated polyesters, epoxy (meth) acrylates, urethane (meth) acrylates, polyester (meth) acrylates, polyether (meth) acrylates, free radical polymerizable monomers, and free radical polymerizable polymers.
[0060] Although crystallinity is omitted, specifically, the above-mentioned crystalline free radical polymerizable compound may contain one or more selected from crystalline unsaturated polyester, crystalline epoxy (meth) acrylate, crystalline urethane (meth) acrylate, crystalline polyester (meth) acrylate, crystalline polyether (meth) acrylate, crystalline free radical polymerizable monomer, and crystalline free radical polymerizable multimer. If these polymerizable compounds are used, mechanical properties and operability are good (crystallinity is sometimes omitted below).
[0061] In addition, in this specification, a crystalline compound can be defined as a compound having a glass transition temperature and a melting point. These temperatures can be confirmed by a thermal analysis device such as DSC (differential scanning calorimeter) and TGDTA (differential thermal thermogravimetric simultaneous determination device). The crystalline compound of the present invention can be used as a compound whose melting point can be confirmed by a thermal analysis device.
[0062] In addition, in a preferred embodiment of the crystalline radical polymerizable composition for sealing electrical and electronic parts of the present invention, it is characterized in that the above-mentioned crystalline radical polymerizable compound has a melting point of 30 to 150°C, more preferably 30 to 120°C, and further preferably 30 to 100°C from the viewpoint of workability and moldability. This is because, compared with the case of using a crystalline radical polymerizable compound with a melting point of less than 30°C or a crystalline radical polymerizable compound with a melting point of more than 150°C, if a crystalline radical polymerizable compound with a melting point in the range of 30 to 150°C is used, better workability can be achieved. When the melting point of the crystalline radical polymerizable compound is lower than the above range, it is easy to become a liquid at room temperature, so there is a concern that the crystalline radical polymerizable composition is not easy to maintain a solid. When the melting point of the crystalline radical polymerizable compound is higher than the above range, it is close to the molding temperature of the mold, so the time from the start of flow to solidification becomes shorter, and there is a concern that molding defects occur.
[0063] In addition, when only a crystalline radical polymerizable compound having a melting point of less than 30° C. is used, there is a tendency for the crystalline radical polymerizable composition to be difficult to solidify at 23° C. On the other hand, when only a crystalline radical polymerizable compound having a melting point of more than 150° C. is used, when the crystalline radical polymerizable composition is plasticized in the cylinder in the injection molding method, the cylinder temperature is close to the temperature of the mold, and thus there is a tendency for the stability in the cylinder to be poor.
[0064] In addition, in a preferred embodiment of the crystalline radical polymerizable composition for sealing electrical and electronic parts of the present invention, it is characterized in that the crystalline radical polymerizable composition is solid at 23°C from the viewpoint of the operability of the crystalline radical polymerizable compound. The above range is set because the shape of the composition does not change under the environment of manufacturing, molding, and transportation of the crystalline radical polymerizable composition, so it can be continuously produced under general manufacturing equipment and conditions. In addition, a solid can be defined as an object whose shape and volume are not easily changed by external force.
[0065] In a preferred embodiment of the crystalline radical polymerizable composition for sealing electrical and electronic parts of the present invention, from the viewpoint of fluidity, the melt viscosity of the crystalline radical polymerizable composition measured by a high-speed flow tester is 90° C. at a measurement temperature of 90° C., a die diameter of 0.5 mm and a length of 1.0 mm, and a pressure of 30 kgf / cm 2 When the pressure is 1kgf / cm 2 When the melt viscosity of the crystalline free radical polymerizable composition is lower than the above range, a lot of thin flashes are generated, and the flashes are not easy to be peeled off from the mold. Furthermore, the composition enters the gap of the mold, making it difficult to continuously mold. When the melt viscosity is higher than the above range, the filling property is poor during molding, and there is a concern that the product cannot be obtained.
[0066] In a preferred embodiment of the crystalline radical polymerizable composition for sealing electrical and electronic parts of the present invention, from the viewpoint of product quality, the inorganic filler can be set to 50 to 95% by weight, more preferably 55 to 93% by weight, and even more preferably 60 to 90% by weight relative to the total amount of the crystalline radical polymerizable composition. The above range is set because when the amount of the inorganic filler is less than the above range, the shrinkage is large and the molded product is deformed, and when it is more than the above range, the melt viscosity during molding is high, which puts a load on the insert and there is a concern that the insert is damaged.
[0067] In addition, in a preferred embodiment of the crystalline free radical polymerizable composition for sealing electrical and electronic parts of the present invention, from the perspective of maintaining solid, the ratio of the crystalline free radical polymerizable compound to the total amount of the free radical polymerizable compound can be set to 30 parts by weight or more, more preferably 40 parts by weight or more, and further preferably 50 parts by weight or more. The above range is set because when the ratio of the crystalline free radical polymerizable compound is less than the above range, there is a concern that it is not easy to become a solid. In addition, the free radical polymerizable compound may include a crystalline free radical polymerizable compound and an amorphous free radical polymerizable compound, and an example of a preferred mode of the ratio of the crystalline free radical polymerizable compound to the total amount of these free radical polymerizable compounds is specified here.
[0068] In addition, in a preferred embodiment of the crystalline radical polymerizable composition for sealing electrical and electronic parts of the present invention, from the viewpoint of quality management of the crystalline radical polymerizable composition, the weight average molecular weight of the crystalline radical polymerizable compound can be set to 100 to 100000, more preferably 100 to 50000, and further preferably 150 to 30000. The above range is set because when the weight average molecular weight of the crystalline radical polymerizable compound is less than the above range, the crystalline radical polymerizable composition is difficult to become a solid, and when it is greater than the above range, the molecular weight of the crystalline radical polymerizable composition cannot be controlled with high precision, so there is a concern that the compound properties and composition properties may vary.
[0069] Furthermore, the sealed electric and electronic component of the present invention is characterized by being sealed with the crystalline radically polymerizable composition for sealing an electric and electronic component of the present invention.
[0070] In addition, the granular material of the present invention is characterized in that it contains the crystalline radical polymerizable composition for sealing electrical and electronic parts of the present invention. Although it is made into granular material, the present invention can also be a powder, a tablet, etc. in addition to the granular material. That is, in the case of other than granular material, the powder, tablet, etc. of the present invention can be composed of the crystalline radical polymerizable composition for sealing electrical and electronic parts of the present invention.
[0071] The method for producing a sealed electric and electronic component of the present invention is characterized by comprising the step of sealing an electric and electronic component by insert molding such as injection molding or transfer molding using the granular material comprising the crystalline radical polymerizable composition for sealing an electric and electronic component of the present invention.
[0072] The sealant for electric and electronic parts is a sealant containing an insert. The sealant for electric and electronic parts is a molded body in which capacitors, integrated circuits, etc. are joined to a substrate and these are covered integrally. The electric and electronic parts joined to the substrate are worried about damage to the electric and electronic parts due to the flow pressure of injection molding or transfer molding using a high-viscosity molding material. In addition, in the present invention, the electric and electronic parts, in addition to the so-called electric and electronic parts, may also include semiconductors, etc. Therefore, these sealants for electric and electronic parts may also be used in semiconductor sealants. In a word, the composition of the present invention can be widely used in sealants requiring operability, fluidity, etc.
[0073] The composition with low melt viscosity and good fluidity is soft even at room temperature, so there is a concern that the operability is poor. In addition, the soft composition becomes a block, and in the case of injection molding, the composition is welded in the feed hopper, and in the case of transfer molding, the previously molded ingots are welded, and then the shape changes, and there is a concern that the ingot cannot enter the ingot insertion hole in the transfer molding machine. The present invention takes into account both fluidity and operability, and can exert an excellent effect of high productivity.
[0074] <Method for producing unsaturated polyester>
[0075] In one example of the unsaturated polyester used in the present invention, for example, by subjecting an unsaturated polyacid, a saturated polyacid and a diol to a known dehydration condensation reaction, the unsaturated polyester can generally have an acid value of 2 to 40 mg-KOH / g. When the unsaturated polyester is produced, the unsaturated polyacid and the saturated polyacid can be selected or combined appropriately, and the diols can be selected or combined, and the proportion thereof can be adjusted to produce a crystalline unsaturated polyester.
[0076] Examples of the unsaturated polybasic acid include maleic acid, maleic anhydride, fumaric acid, citraconic acid, mesaconic acid, itaconic acid, tetrahydrophthalic acid, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, and glutaconic acid.
[0077] Examples of the saturated polybasic acids include phthalic acid, phthalic anhydride, isophthalic acid, terephthalic acid, succinic acid, adipic acid, sebacic acid, azelaic acid, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, endomethylenetetrahydrophthalic anhydride, chlorobridgeic acid, and tetrabromophthalic anhydride.
[0078] Examples of the diols include ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, propylene glycol, diethylene glycol, triethylene glycol, dipropylene glycol, neopentyl glycol, 1,3-butanediol, hydrogenated bisphenol A, bisphenol A propylene oxide compounds, cyclohexanedimethanol, and dibromoneopentyl glycol.
[0079] In the present invention, among the crystalline unsaturated polyesters, unsaturated polyesters using fumaric acid as the unsaturated polybasic acid, using isophthalic acid or terephthalic acid as the saturated polybasic acid, and mainly using ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, or cyclohexanedimethanol as the diol are preferred.
[0080] <Method for producing epoxy (meth)acrylate>
[0081] The epoxy (meth) acrylate used in the present invention can be produced according to a known method. In the presence or absence of a known inhibitor (prohibitor) and a known esterification catalyst, in an inert gas stream or in an air environment, by appropriately selecting an epoxy resin and an unsaturated monobasic acid, a crystalline epoxy (meth) epoxy acrylate can be produced. In order to reduce the melt viscosity of the reaction system as required, other free radical polymerizable monomers or organic solvents can be added to react.
[0082] As for the epoxy (meth) acrylate of the present invention, as an example, it can be an epoxy (meth) acrylate having a double bond of acrylate or methacrylate at the molecular end obtained by addition reaction of an epoxy resin having two or more glycidyl ether groups in one molecule with acrylic acid or methacrylic acid. It can also be an epoxy (meth) acrylate resin in which epoxy (meth) acrylate is dissolved in a radical polymerizable monomer and / or a radical polymerizable multimer. The epoxy resin having two or more glycidyl ether groups in one molecule can be, for example, bisphenol-type epoxy resins from bisphenol A, bisphenol F, bisphenol S, or derivatives thereof, biphenol-type epoxy resins from biphenol and its derivatives, biphenol-type epoxy resins from biphenol and its derivatives, or naphthalene-type epoxy resins from naphthalene and its derivatives, and epoxy resins such as novolac-type epoxy resins, which can be used alone or in combination of two or more. The epoxy equivalent, which is an index of the molecular weight of the epoxy resin, is preferably 174 to 2000 eq / g.
[0083] <Method for producing urethane (meth)acrylate>
[0084] In addition, as for the urethane (meth) acrylate of the present invention, as an example, it can be an isocyanate at the molecular end obtained by reacting a polyol and / or polyester polyol and / or polyether polyol having two or more hydroxyl groups in one molecule with a diisocyanate, and / or a compound having an alcoholic hydroxyl group and one or more acrylate groups or methacrylate groups in one molecule, or a urethane acrylate having an acrylate or methacrylate double bond at the molecular end obtained by first reacting a compound having an alcoholic hydroxyl group and one or more acrylate groups or methacrylate groups with a diisocyanate in such a way that an isocyanate group remains, and then reacting the remaining isocyanate group with a polyol and / or polyester polyol and / or polyether polyol having two or more hydroxyl groups in one molecule. When manufacturing carbamate (meth) acrylate, by appropriately selecting a combination of isocyanate, polyol and / or polyester polyol and / or polyether polyol, and a compound having an alcoholic hydroxyl group and one or more acrylate groups or methacrylate groups, a carbamate (meth) epoxy acrylate having crystallinity can be prepared. It can also be a carbamate (meth) acrylate resin in which carbamate acrylate or carbamate methacrylate is dissolved in a free radical polymerizable monomer and / or free radical polymerizable multimer such as styrene and diethylene glycol dimethacrylate. These can be used alone or in a mixture of two or more.
[0085] The above-mentioned compound having an alcoholic hydroxyl group and one or more acrylate groups or methacrylate groups may be hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, phenoxyhydroxypropyl (meth)acrylate, trimethylolpropane di(meth)acrylate, dipropylene glycol mono(meth)acrylate, or the like.
[0086] In addition, the polyol having two or more hydroxyl groups in one molecule may be used alone or in combination of two or more thereof, such as neopentyl glycol, ethylene glycol, 1,3-propylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, propylene glycol, diethylene glycol, dipropylene glycol, trimethylene glycol, hydrogenated bisphenol A, bisphenol A ethylene oxide adduct, bisphenol A propylene oxide adduct, etc. The polyester polyol having two or more hydroxyl groups in one molecule may be used alone or in combination of two or more thereof, such as neopentyl glycol, ethylene glycol, A saturated polyester polyol with a molecular weight of 1000 to 2000 obtained by the dehydration condensation reaction of a polyol such as propylene glycol, diethylene glycol, dipropylene glycol, trimethylene glycol, hydrogenated bisphenol A, bisphenol A ethylene oxide adduct, bisphenol A propylene oxide adduct and a polybasic acid such as adipic acid, phthalic acid (anhydride), isophthalic acid, terephthalic acid, trimellitic acid, etc.; the above-mentioned polyether polyol having two or more hydroxyl groups in one molecule can be used alone or in combination of two or more polyethylene glycols with a molecular weight of 300 to 2000 obtained by the ring-opening reaction of ethylene oxide or propylene oxide, polypropylene glycols, or polycaprolactone obtained by the ring-opening reaction of caprolactone, etc.
[0087] As the compound having two or more isocyanate groups in one molecule, aromatic and / or aliphatic polyisocyanate compounds can be used, for example, toluene diisocyanate, diphenylmethane diisocyanate, hydrogenated diphenylmethane diisocyanate, 1,6-hexamethylene diisocyanate, isophorone diisocyanate, xylene diisocyanate, hydrogenated xylene diisocyanate, trifunctional isocyanate having an isocyanurate ring formed by trimerization of a bifunctional isocyanate compound, commercially available polyol-modified isocyanate prepolymers, etc. These can be used alone or in combination of two or more.
[0088] <Method for producing polyester (meth)acrylate>
[0089] In addition, as for the polyester (meth) acrylate of the present invention, as an example, it can be a polyester acrylate or polyester methacrylate having a double bond of acrylate or methacrylate at the molecular end obtained by esterification of polyester polyol with acrylic acid or methacrylate, or reaction of acid-terminated polyester with acrylate or methacrylate having glycidyl group. When manufacturing polyester (meth) acrylate, by appropriately selecting polyester polyol and acrylic acid or methacrylate, or acid-terminated polyester and acrylate or methacrylate having glycidyl group, a crystalline polyester (meth) acrylate can be prepared. It can also be a polyester acrylate resin or polyester methacrylate resin in which polyester acrylate or polyester methacrylate is dissolved in a free radical polymerizable monomer and / or free radical polymerizable multimer such as styrene, diethylene glycol dimethacrylate, etc. These can be used alone or as a mixture of two or more.
[0090] <Method for producing polyether (meth)acrylate>
[0091] In addition, the polyether (meth) acrylate of the present invention, as an example, can be a polyether acrylate or polyether methacrylate having a double bond of acrylate or methacrylate at the molecular end obtained by esterification of polyether polyol and acrylic acid or methacrylic acid, or reaction of acid-terminated polyether and acrylate or methacrylate having glycidyl group. When manufacturing polyether (meth) acrylate, by appropriately selecting polyether polyol and acrylic acid or methacrylic acid, or acid-terminated polyester and acrylate or methacrylate having glycidyl group, a crystalline polyester (meth) acrylate can be made. It can also be a polyether acrylate resin or polyether methacrylate resin in which polyether acrylate or polyether methacrylate is dissolved in a free radical polymerizable monomer and / or free radical polymerizable multimer such as styrene, diethylene glycol dimethacrylate, etc. These can be used alone or as a mixture of two or more.
[0092] In a preferred embodiment, the crystalline radical polymerizable monomer that is solid at 30 to 150° C. in the present invention may contain ethoxylated isocyanuric acid triacrylate (melting point about 50° C.), polyethylene glycol di(meth)acrylate (melting point 35 to 53° C.), methoxy polyethylene glycol (meth)acrylate (melting point 33 to 40° C.), behenyl acrylate (melting point 46° C.), tetramethylpiperidinyl methacrylate (melting point 56 to 60° C.), trimethylallyl isocyanurate (melting point 83-87°C), diacetone acrylamide (melting point about 56°C), dimethyl itarate (melting point 36°C), vinyl stearate (melting point 36°C), N-vinyl carbazole (melting point 67°C), N-hydroxymethyl acrylamide (melting point 71-75°C), acrylamide (melting point 84°C), tolylidene diallyl carbamate (melting point 85-110°C), maleimide (melting point 93°C), acenaphthylene (melting point 95°C), etc. One or more. When these crystalline free radical polymerizable compounds are used, the workability is good.
[0093] As for the radical polymerizable monomer of the present invention, a radical polymerizable monomer that is liquid at room temperature can be used within the scope that does not impair the purpose of the present invention. Examples thereof include vinyl aromatic compounds such as styrene monomer, α-methylstyrene, vinyltoluene, α-chlorostyrene, etc. having a vinyl group; vinyl esters such as vinyl acetate, vinyl propionate, vinyl lactate, vinyl butyrate, VeoVa monomer (manufactured by Shell Chemical Co.); (meth)acrylates such as methyl acrylate, ethyl acrylate, n-butyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, etc.
[0094] In addition, free radical polymerizable monomers having two or more functions such as triallyl cyanurate, diethylene glycol dimethacrylate, diallyl tetrabromophthalate, phenoxyethyl acrylate, 2-hydroxyethyl acrylate, 1,6-hexanediol diacrylate, diallyl phthalate having an allyl group, and triallyl isocyanurate can also be used. These free radical polymerizable monomers can be used alone or in combination of two or more.
[0095] As the radical polymerizable multimer of the present invention, diallyl phthalate prepolymer, TAIC prepolymer, epoxy prepolymer, urethane prepolymer, acrylate prepolymer can be used. These radical polymerizable multimers can be used alone or in combination of two or more.
[0096] In the crystalline free radical polymerizable composition for sealing electrical and electronic parts of the present invention, an inorganic filler can be used. The inorganic filler can include calcium carbonate, magnesium carbonate, barium carbonate, calcium hydroxide, aluminum hydroxide, magnesium hydroxide, magnesium oxide, aluminum oxide, silicon dioxide, zinc oxide, mica, aluminum nitride, and boron nitride. Among these, silicon dioxide is preferred from the viewpoint of fluidity. These can be used alone or in combination of two or more.
[0097] The inorganic filler may have an average particle size of 100 μm or less, preferably 0.01 to 50 μm. By using an inorganic filler having such an average particle size, a crystalline radical polymerizable composition for sealing electric and electronic parts having excellent fluidity and strength during molding can be prepared.
[0098] The crystalline radical polymerizable composition for sealing electric and electronic parts of the present invention may be blended with various additives that are closely coupled with the inorganic filler and the reinforcing material, for example, a (meth)acrylate compound having a polar group or a coupling agent.
[0099] The (meth)acrylate compound having a polar group is not particularly limited, and examples thereof include (meth)acrylate compounds containing substituents containing atoms other than carbon and hydrogen to form ester bonds, and examples of substituents include hydroxyl, epoxy, glycidyl, tetrahydrofuranyl, isocyanate, carboxyl, alkoxysilyl, phosphate, lactone, oxetane, tetrahydropyranyl, amino, etc. The coupling agent is not particularly limited, and examples thereof include silane coupling agents and titanate coupling agents, and examples of silane coupling agents include epoxy silane, amino silane, cationic silane, vinyl silane, acrylic silane, mercapto silane, and composites thereof.
[0100] Among these, acrylic silane coupling agents are preferred from the viewpoint of improving strength. In addition, various additives may be used without impairing the purpose of the present invention.
[0101] In the crystalline radical polymerizable composition for sealing electric and electronic parts of the present invention, as a radical polymerization initiator, a thermally decomposable organic peroxide or a polymerization inhibitor which is usually used for unsaturated polyester resin compositions and radical polymerizable compositions can be used.
[0102] Examples of the organic peroxide include tert-butyl peroxy-2-ethylhexyl monocarbonate, 1,1-di(tert-hexylperoxy)cyclohexane, 1,1-di(tert-butylperoxy)-3,3,5-trimethylcyclohexane, tert-butyl peroxyoctanoate, benzoyl peroxide, methyl ethyl ketone peroxide, acetylacetone peroxide, tert-butyl peroxybenzoate, diisopropylbenzene peroxide, etc. These may be used alone or in combination of two or more.
[0103] Among these, from the viewpoint of molding conditions and storage stability, it is preferable to use an organic peroxide having a 10-hour half-life temperature of 100° C. or higher. Specifically, dicumyl peroxide is preferably used.
[0104] Examples of the polymerization inhibitor include hydroquinone, monomethyl ether hydroquinone, methyl hydroquinone, di-t-4-methylphenol, monomethyl ether hydroquinone, phenothiazine, tert-butylcatechol, p-benzoquinone, quinones such as gallol, 2,6-di-tert-butyl-p-cresol, 2,2-methylene-bis-(4-methyl-6-tert-butylphenol), 1,1,3-tris-(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, Piperidine-1-oxy free radicals such as 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxy free radical, 4-oxo-2,2,6,6-tetramethylpiperidin-1-oxy free radical, 4-methoxy-2,2,6,6-tetramethylpiperidin-1-oxy free radical, 4-carboxyl-2,2,6,6-tetramethylpiperidin-1-oxy free radical, and 2,2,6,6-tetramethylpiperidin-1-oxy free radical. By using these, thickening during the filling period during molding can be suppressed, and a free radical polymerizable composition with low melt viscosity can be prepared. These can be used alone or in combination of two or more.
[0105] The crystalline radical polymerizable composition for sealing electric and electronic parts of the present invention may contain a reinforcing material. By using the reinforcing material, the crystalline radical polymerizable composition for sealing electric and electronic parts having excellent strength characteristics and dimensional stability can be obtained.
[0106] As the reinforcing material used in the present invention, glass fiber generally used in fiber-reinforced plastics such as BMC (bulk molding compound) and SMC (sheet molding compound) can be used, but the material is not limited to glass fiber and other materials may be used.
[0107] As glass fibers, there can be mentioned glass fibers such as E glass (alkali-free glass for electrical use), C glass (alkali-containing glass for chemical use), A glass (acid-resistant glass), and S glass (high-strength glass) made of silicate glass and borosilicate glass, and articles made of these into long fibers (rovings), short fibers (chopped strands), and ground fibers can also be used. In addition, articles that have been subjected to surface treatment can also be used for these glass fibers.
[0108] Furthermore, the crystalline radically polymerizable composition for sealing electric and electronic parts of the present invention may contain other inorganic fillers as appropriate within a range that does not inhibit the fluidity of the composition or the properties of the sealing material.
[0109] Examples of these materials include oxides and hydrates thereof, inorganic foamed particles, and hollow particles such as silica balloons.
[0110] In the crystalline free radical polymerizable composition for sealing electrical and electronic parts of the present invention, a release agent can be used. As a release agent, a fatty acid system, a fatty acid metal salt system, a mineral system, etc. waxes used in general thermosetting resins can be used, and it is particularly preferred to use a fatty acid system, a fatty acid metal salt system, and waxes with excellent heat discoloration resistance.
[0111] Specific examples of these release agents include stearic acid, zinc stearate, aluminum stearate, calcium stearate, paraffin, etc. These release agents may be used alone or in combination of two or more.
[0112] As the mold release agent, an external mold release agent such as a mold release agent that is sprayed or applied to a mold, or a molding material containing a mold release agent may be used as necessary.
[0113] In the present invention, in addition to these ingredients, a curing catalyst, a polymerization inhibitor, a colorant, a thickener, a wetting and dispersing agent, a surface conditioner, a viscosity reducing agent, a flow modifier, other organic additives, inorganic additives, etc. for adjusting the curing conditions of the crystalline free radical polymerizable composition can be appropriately formulated as needed.
[0114] <Method for producing crystalline radical polymerizable composition>
[0115] The crystalline radical polymerizable composition for sealing electric and electronic parts of the present invention can be produced by blending the components using a stirrer, blender or the like, mixing them sufficiently and uniformly, and then preparing and granulating them using a kneading machine, extruder or the like capable of heating and pressurizing.
[0116] The granular material, powder, and ingot of the present invention are characterized by being composed of the crystalline radical polymerizable composition for sealing electric and electronic parts of the present invention. The granular material formed from the crystalline radical polymerizable composition for sealing electric and electronic parts of the present invention may be in the form of granules.
[0117] In addition, the electric and electronic component sealed body of the present invention is characterized in that granules, powders, and tablets formed from the crystalline free radical polymerizable composition for sealing electric and electronic components of the present invention are molded and sealed. The electric and electronic component sealed body can be molded by various molding methods of thermosetting compositions according to conventional methods.
[0118] The crystalline radical polymerizable composition for sealing electric and electronic parts of the present invention is dry and has good thermal stability when melted, so it is suitable for molding using melt heating molding methods such as injection molding, injection compression molding, transfer molding, and compression molding.
[0119] Among these, injection molding using an injection molding machine and transfer molding using a transfer molding machine are particularly suitable. Injection molding can shorten the molding time, and transfer molding can mold multiple molded bodies at a time, so that electric and electronic parts sealed bodies with complex shapes can be manufactured.
[0120] <Electrical and electronic component sealed body and method for manufacturing the same>
[0121] The electric and electronic component sealed body of the present invention can be manufactured by sealing the electric and electronic component by insert molding using the crystalline radical polymerizable composition for electric and electronic component sealing of the present invention. Here, the crystalline radical polymerizable composition for electric and electronic component sealing of the present invention may be a composition in which all components constituting the crystalline radical polymerizable composition are separately preheated and kneaded, or a composition in which a part or all of the components are mixed just before injection into a mold and then heated and kneaded.
[0122] The temperature and pressure of the crystalline free radical polymerizable composition during mold injection are not particularly limited. When an injection molding machine is used, if the temperature of the crystalline free radical polymerizable composition is 60 to 130° C., the mold temperature is 130 to 190° C., and the pressure of the crystalline free radical polymerizable composition is 0.1 to 10 MPa, and in the case of a transfer molding machine, the mold temperature is set to 130 to 190° C. and the pressure of the crystalline free radical polymerizable composition is set to 0.1 to 10 MPa, then damage to electrical and electronic parts is reduced, which is preferred.
[0123] Next, an example of the crystalline radical polymerizable composition for electric and electronic components of the present invention will be described as follows.
[0124] The crystalline radical polymerizable composition for electrical and electronic parts of the present invention is characterized in that it contains at least a crystalline radical polymerizable compound, an inorganic filler, a silane coupling agent, and a radical polymerization initiator. This is because by using the crystalline radical polymerizable composition, as shown in the examples described below, a polymerizable composition with excellent thermal conductivity and workability can be achieved. In addition, in this specification, the crystalline radical polymerizable composition for electrical and electronic parts is sometimes referred to as a crystalline radical polymerizable composition.
[0125] In addition, in a preferred embodiment of the crystalline free radical polymerizable composition for electrical and electronic parts of the present invention, it is characterized in that the thermal conductivity of the molded body molded from the crystalline free radical polymerizable composition for electrical and electronic parts is 1.0 W / m·K or more. The above range is set because from the perspective of heat release, if it is less than 1.0 W / m·K, the thermal conductivity is low, and there is a concern that the electrical and electronic parts will accumulate heat and fail. In the past, in order to improve thermal conductivity, a thermally conductive filler with concave and convex was generally used, but a molding material with a high thermal conductivity is compounded with a large amount of thermally conductive filler, so the fluidity is reduced, the use is limited, and there is a tendency for the price to increase. However, it is found that according to the present invention, a sufficiently high thermal conductivity can be obtained, and the fluidity is also good, and the usability is excellent.
[0126] In addition, in a preferred embodiment of the crystalline free radical polymerizable composition for electrical and electronic parts of the present invention, the above-mentioned crystalline free radical polymerizable compound may contain one or more selected from unsaturated polyesters, epoxy (meth) acrylates, urethane (meth) acrylates, polyester (meth) acrylates, polyether (meth) acrylates, free radical polymerizable monomers, and free radical polymerizable polymers.
[0127] Although crystallinity is omitted, specifically, the above-mentioned crystalline free radical polymerizable compound may contain one or more selected from crystalline unsaturated polyester, crystalline epoxy (meth) acrylate, crystalline urethane (meth) acrylate, crystalline polyester (meth) acrylate, crystalline polyether (meth) acrylate, crystalline free radical polymerizable monomer, and crystalline free radical polymerizable multimer. If these polymerizable compounds are used, mechanical properties and operability are good (crystallinity is sometimes omitted below).
[0128] In addition, in this specification, the above-mentioned crystalline free radical polymerizable compound is also included, and the crystalline compound can be defined as a compound having a glass transition temperature and a melting point. These temperatures can be confirmed by a thermal analysis device such as DSC (differential scanning calorimeter) and TGDTA (differential thermal thermogravimetric simultaneous determination device). The crystalline compound of the present invention can be used as a compound that can confirm the melting point by a thermal analysis device.
[0129] In addition, in a preferred embodiment of the crystalline radical polymerizable composition for electrical and electronic parts of the present invention, the melting point of the crystalline radical polymerizable compound is preferably 30 to 150°C, and more preferably 30 to 120°C from the viewpoint of workability and moldability. This is because, compared with the case of using a crystalline radical polymerizable compound with a melting point of less than 30°C or a crystalline radical polymerizable compound with a melting point of more than 150°C, a crystalline radical polymerizable compound with a melting point in the range of 30 to 150°C can achieve better workability. When the melting point of the crystalline radical polymerizable compound is lower than the above range, it is easy to become a liquid at room temperature, so there is a concern that the crystalline radical polymerizable composition is not easy to maintain a solid. When the melting point of the crystalline radical polymerizable compound is higher than the above range, since it is close to the molding temperature of the mold, the time from the start of flow to solidification becomes shorter, and there is a concern that molding defects may occur.
[0130] In addition, when only a crystalline radical polymerizable compound having a melting point of less than 30° C. is used, there is a tendency that the crystalline radical polymerizable composition is not easily solidified at 23° C. On the other hand, when only a crystalline radical polymerizable compound having a melting point of more than 150° C. is used, when the crystalline radical polymerizable composition is plasticized in the cylinder in the injection molding method, the cylinder temperature is close to the mold temperature, so there is a concern that the curing reaction in the cylinder proceeds, and there is a tendency to lack stability.
[0131] In addition, in a preferred embodiment of the crystalline radical polymerizable composition for electrical and electronic parts of the present invention, the crystalline radical polymerizable composition is preferably solid at 23°C from the viewpoint of the operability of the crystalline radical polymerizable compound. The above range is set because the shape of the composition does not change under the environment of manufacturing, molding, and transportation of the crystalline radical polymerizable composition, so it can be continuously produced under general manufacturing equipment and conditions. In addition, a solid can be defined as an object whose shape and volume are not easily changed by external force.
[0132] In a preferred embodiment of the crystalline radical polymerizable composition for electrical and electronic parts of the present invention, from the viewpoint of product quality, the inorganic filler can be set to 40 to 95% by weight, more preferably 50 to 93% by weight, and even more preferably 60 to 90% by weight relative to the total amount of the crystalline radical polymerizable composition. The above range is set because when the amount of the inorganic filler is less than the above range, the shrinkage is large and the molded product is deformed, and when it is more than the above range, the melt viscosity during molding is high, and there is a concern that the molded product may not be filled or part of the molded product may be gas-burned and carbonized.
[0133] In addition, in a preferred embodiment of the crystalline free radical polymerizable composition for electrical and electronic parts of the present invention, from the viewpoint of maintaining solid, the ratio of the above-mentioned crystalline free radical polymerizable compound to the total amount of free radical polymerizable compounds can be set to 25 parts by weight or more, more preferably 30 parts by weight or more, and further preferably 35 parts by weight or more. The above range is set because when the ratio of the crystalline free radical polymerizable compound is less than the above range, there is a concern that it is not easy to become a solid. In the case of the composition of the present invention, it can become a high viscosity, so the degree of freedom can be increased to a certain extent. In addition, the free radical polymerizable compound may include a crystalline free radical polymerizable compound and an amorphous free radical polymerizable compound, and an example of a suitable manner of the ratio of the crystalline free radical polymerizable compound to the total amount of these free radical polymerizable compounds is specified here.
[0134] In addition, in a preferred embodiment of the crystalline radical polymerizable composition for electrical and electronic parts of the present invention, from the viewpoint of quality management of the crystalline radical polymerizable composition, the weight average molecular weight of the crystalline radical polymerizable compound can be set to 70 to 100,000, more preferably 100 to 50,000, and even more preferably 150 to 30,000. The above range is set because when the weight average molecular weight of the crystalline radical polymerizable compound is less than the above range, there is a concern that the crystalline radical polymerizable composition is not easy to become a solid, and when it is greater than the above range, the molecular weight of the crystalline radical polymerizable composition cannot be controlled with high precision, so there is a concern that the compound properties and composition properties vary.
[0135] In a preferred embodiment of the electric and electronic component molded body of the present invention, the molded body is molded from the crystalline radical polymerizable composition for an electric and electronic component of the present invention.
[0136] In a preferred embodiment of the electric and electronic component molded body of the present invention, the thermal conductivity of the molded body is 1.0 W / m·K or more. The above range is set because, from the viewpoint of heat dissipation, if it is less than 1.0 W / m·K, the thermal conductivity is low, and the electric and electronic components may accumulate heat and fail.
[0137] In addition, in a preferred embodiment of the granular material of the present invention, it is composed of the crystalline free radical polymerizable composition for electric and electronic parts of the present invention. Although it is made into a granular material, the present invention can also be a powder, a flake, a granule, etc. in addition to a granular material. That is, in the case of a granular material, the powder, flake, granule, etc. of the present invention can be composed of the crystalline free radical polymerizable composition for electric and electronic parts of the present invention.
[0138] In addition, in a preferred embodiment of the method for producing an electric and electronic component molded body of the present invention, there is a step of molding the granular material comprising the crystalline radical polymerizable composition for electric and electronic components of the present invention into an electric and electronic component molded body by injection molding, transfer molding, compression molding, or hot melt molding. Injection molding allows production in a short time, and transfer molding allows a large number of products to be obtained at one time.
[0139] The electric and electronic parts molded body of the present invention may contain an insert. The electric and electronic parts molded body can be made into an insert molded body of a housing of an electric and electronic part, a metal of an electric and electronic part, and / or a coil. Due to the flow pressure of injection molding or transfer molding using a high-viscosity molding material, there is a concern that the electric and electronic parts may be damaged. In addition, in the present invention, the electric and electronic parts, in addition to the so-called electric and electronic parts, may also include semiconductors, etc. Therefore, these electric and electronic parts molded bodies can also be used in semiconductor sealed bodies. In short, the composition of the present invention can be widely used in molded bodies that require high thermal conductivity, usability, etc.
[0140] As for the composition with low melt viscosity and good fluidity, the composition is soft even at room temperature, so there is a concern about poor operability. In addition, the soft composition becomes a block, and in the case of injection molding, the composition is welded in the feed hopper, and in the case of transfer molding, the previously molded ingots are welded, and then the shape changes, and there is a concern that the ingot cannot enter the ingot insertion hole in the transfer molding machine. The present invention takes into account both fluidity and operability, and can exert an excellent effect of high productivity.
[0141] <Method for producing unsaturated polyester>
[0142] The unsaturated polyester used in the present invention can have an acid value of 2 to 40 mg-KOH / g by subjecting unsaturated polyacids, saturated polyacids and diols to a known dehydration condensation reaction. When producing the unsaturated polyester, the unsaturated polyacid and the saturated polyacid can be selected or combined appropriately, and the diols can be selected or combined, and the proportion thereof can be selected to produce a crystalline unsaturated polyester.
[0143] Examples of the unsaturated polybasic acid include maleic acid, maleic anhydride, fumaric acid, citraconic acid, mesaconic acid, itaconic acid, tetrahydrophthalic acid, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, and glutaconic acid.
[0144] Examples of the saturated polybasic acids include phthalic acid, phthalic anhydride, isophthalic acid, terephthalic acid, succinic acid, adipic acid, sebacic acid, azelaic acid, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, endomethylenetetrahydrophthalic anhydride, chlorobridgeic acid, tetrabromophthalic anhydride, 1,4-cyclohexanedicarboxylic acid, 2,6-naphthalene dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 2,3-naphthalene dicarboxylic acid, 1,5-naphthalene dicarboxylic acid, and 1,8-naphthalene dicarboxylic acid.
[0145] Examples of the diols include ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, propylene glycol, diethylene glycol, triethylene glycol, dipropylene glycol, neopentyl glycol, 1,3-butanediol, hydrogenated bisphenol A, bisphenol A propylene oxide compound, cyclohexanedimethanol, dibromoneopentyl glycol, isosorbide, isomannide, and tricyclodecane dimethanol.
[0146] In the present invention, even among crystalline unsaturated polyesters, unsaturated polyesters using fumaric acid as the unsaturated polybasic acid, isophthalic acid or terephthalic acid as the saturated polybasic acid, and mainly using ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, or 1,4-cyclohexanedimethanol as the diol are preferred.
[0147] <Method for producing epoxy (meth)acrylate>
[0148] The epoxy (meth) acrylate used in the present invention can be produced according to a method known per se. Crystalline epoxy (meth) epoxy acrylate can be produced by appropriately selecting epoxy resin and unsaturated monobasic acid in the presence or absence of a known inhibitor or a known esterification catalyst in an inert gas stream or in an air environment. In order to reduce the melt viscosity of the reaction system as required, other free radical polymerizable monomers or organic solvents can be added to react.
[0149] As for the epoxy (meth) acrylate in the present invention, as an example, it can be an epoxy (meth) acrylate having a double bond of acrylate or methacrylate at the molecular end obtained by, for example, an epoxy resin having two or more glycidyl ether groups in one molecule and acrylic acid or methacrylic acid. It can also be an epoxy (meth) acrylate resin in which epoxy (meth) acrylate is dissolved in a free radical polymerizable monomer and / or a free radical polymerizable multimer. As for the epoxy resin having two or more glycidyl ether groups in one molecule, for example, epoxy resins such as bisphenol A, bisphenol F, bisphenol S, or derivatives thereof, biphenol-type epoxy resins from biphenyl and its derivatives, biphenol-type epoxy resins from biphenol and its derivatives, or naphthalene-type epoxy resins from naphthalene and its derivatives, novolac-type epoxy resins, and aliphatic epoxy resins can be cited, and these can be used alone or in combination of two or more. The epoxy equivalent which is an index of the molecular weight of the epoxy resin is preferably 125 to 4,000 eq / g.
[0150] <Method for producing urethane (meth)acrylate>
[0151] In addition, as for the urethane (meth) acrylate in the present invention, as an example, it can be an isocyanate at the molecular end obtained by reacting a polyol and / or polyester polyol and / or polyether polyol having two or more hydroxyl groups in one molecule with a diisocyanate, and / or a compound having an alcoholic hydroxyl group and one or more acrylate groups or methacrylate groups in one molecule, or first reacting a compound having an alcoholic hydroxyl group and one or more acrylate groups or methacrylate groups with a diisocyanate so that an isocyanate group remains, and then reacting the remaining isocyanate group with a polyol and / or polyester polyol and / or polyether polyol having two or more hydroxyl groups in one molecule, to obtain a urethane acrylate having an acrylate or methacrylate double bond at the molecular end. When manufacturing carbamate (meth) acrylate, by appropriately selecting a combination of isocyanate, polyol and / or polyester polyol and / or polyether polyol, and a compound having an alcoholic hydroxyl group and one or more acrylate groups or methacrylate groups, a carbamate (meth) epoxy acrylate having crystallinity can be prepared. It can also be a carbamate (meth) acrylate resin in which carbamate acrylate or carbamate methacrylate is dissolved in a free radical polymerizable monomer and / or free radical polymerizable multimer such as styrene and diethylene glycol dimethacrylate. These can be used alone or in a mixture of two or more.
[0152] The above-mentioned compound having an alcoholic hydroxyl group and one or more acrylate groups or methacrylate groups may include hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, phenoxyhydroxypropyl (meth)acrylate, trimethylolpropane di(meth)acrylate, dipropylene glycol mono(meth)acrylate, and the like.
[0153] In addition, as the polyol having two or more hydroxyl groups in one molecule, for example, neopentyl glycol, ethylene glycol, 1,3-propylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, propylene glycol, diethylene glycol, dipropylene glycol, trimethylene glycol, hydrogenated bisphenol A, bisphenol A ethylene oxide adduct, bisphenol A propylene oxide adduct, etc. can be used. The polyester polyol having two or more hydroxyl groups in one molecule can be composed of neopentyl glycol, ethylene glycol, propylene glycol, diethylene glycol, A saturated polyester polyol having a molecular weight of 400 to 2,000 obtained by a dehydration condensation reaction of a polyhydric alcohol such as dipropylene glycol, trimethylene glycol, hydrogenated bisphenol A, bisphenol A ethylene oxide adduct, bisphenol A propylene oxide adduct and the like with a polybasic acid such as adipic acid, phthalic acid (anhydride), isophthalic acid, terephthalic acid, trimellitic acid and the like. The polyether polyol having two or more hydroxyl groups in one molecule can use polyethylene glycol or polypropylene glycol having a molecular weight of 300 to 4,000 obtained by a ring-opening reaction of ethylene oxide or propylene oxide, or polycaprolactone obtained by a ring-opening reaction of caprolactone, and the like, and can be used alone or in combination of two or more.
[0154] As the compound having two or more isocyanate groups in one molecule, aromatic and / or aliphatic polyisocyanate compounds can be used, for example, toluene diisocyanate, diphenylmethane diisocyanate, hydrogenated diphenylmethane diisocyanate, 1,6-hexamethylene diisocyanate, isophorone diisocyanate, xylene diisocyanate, hydrogenated xylene diisocyanate, trifunctional isocyanate having an isocyanurate ring formed by trimerization of a bifunctional isocyanate compound, isocyanate prepolymers modified with biuret, adducts, and commercially available polyols, etc. These can be used alone or in combination of two or more.
[0155] <Method for producing polyester (meth)acrylate>
[0156] In addition, as for the polyester (meth) acrylate in the present invention, as an example, it can be a polyester acrylate or polyester methacrylate having a double bond of acrylate or methacrylate at the molecular end obtained by esterification of polyester polyol with acrylic acid or methacrylate, or reaction of acid-terminated polyester with acrylate or methacrylate having glycidyl group. When manufacturing polyester (meth) acrylate, by appropriately selecting polyester polyol and acrylic acid or methacrylate, or acid-terminated polyester and acrylate or methacrylate having glycidyl group, a crystalline polyester (meth) acrylate can be prepared. It can also be a polyester acrylate resin or polyester methacrylate resin in which polyester acrylate or polyester methacrylate is dissolved in a free radical polymerizable monomer and / or free radical polymerizable multimer such as styrene, diethylene glycol dimethacrylate, etc. These can be used alone or as a mixture of two or more.
[0157] <Method for producing polyether (meth)acrylate>
[0158] In addition, as for the polyether (meth) acrylate in the present invention, as an example, it can be a polyether acrylate or polyether methacrylate having a double bond of acrylate or methacrylate at the molecular end obtained by esterification of polyether polyol and acrylic acid or methacrylic acid, or reaction of acid-terminated polyether and acrylate or methacrylate having glycidyl group. When manufacturing polyether (meth) acrylate, by appropriately selecting polyether polyol and acrylic acid or methacrylic acid, or acid-terminated polyester and acrylate or methacrylate having glycidyl group, a crystalline polyester (meth) acrylate can be made. It can also be a polyether acrylate resin or polyether methacrylate resin in which polyether acrylate or polyether methacrylate is dissolved in a free radical polymerizable monomer and / or free radical polymerizable multimer such as styrene, diethylene glycol dimethacrylate, etc. These can be used alone or as a mixture of two or more.
[0159] In a preferred embodiment, the crystalline radical polymerizable monomer which is solid at 30 to 150° C. in the present invention may contain ethoxylated isocyanuric acid triacrylate (melting point about 50° C.), polyethylene glycol di(meth)acrylate (melting point 35 to 53° C.), methoxy polyethylene glycol (meth)acrylate (melting point 33 to 40° C.), behenyl acrylate (melting point 46° C.), tetramethylpiperidinyl methacrylate (melting point 56 to 60° C.), isocyanuric acid triacrylate (melting point about 50° C.), polyethylene glycol di(meth)acrylate (melting point 35 to 53° C.), methoxy polyethylene glycol (meth)acrylate (melting point 33 to 40° C.), behenyl acrylate (melting point 46° C.), tetramethylpiperidinyl methacrylate (melting point 56 to 60° C.), At least one of methallyl ester (melting point 83-87°C), diacetone acrylamide (melting point about 56°C), dimethyl itaconate (melting point 36°C), vinyl stearate (melting point 36°C), N-vinyl carbazole (melting point 67°C), N-hydroxymethyl acrylamide (melting point 71-75°C), acrylamide (melting point 84°C), tolylidene diallyl carbamate (melting point 85-110°C), maleimide (melting point 93°C), acenaphthylene (melting point 95°C), etc. When these crystalline free radical polymerizable compounds are used, the workability is good.
[0160] As for the radical polymerizable monomer in the present invention, a radical polymerizable monomer that is liquid at room temperature can be used within the scope that does not impair the purpose of the present invention. Examples thereof include vinyl aromatic compounds such as styrene monomer, α-methylstyrene, vinyltoluene, α-chlorostyrene, etc. having a vinyl group; vinyl esters such as vinyl acetate, vinyl propionate, vinyl lactate, vinyl butyrate, VeoVa monomer (manufactured by Shell Chemical Co.); (meth)acrylates such as methyl acrylate, ethyl acrylate, n-butyl acrylate, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, etc.
[0161] In addition, free radical polymerizable monomers having two or more functions such as triallyl cyanurate, diethylene glycol dimethacrylate, diallyl tetrabromophthalate, phenoxyethyl acrylate, 2-hydroxyethyl acrylate, 1,6-hexanediol diacrylate, diallyl phthalate having an allyl group, diallyl maleate, diallyl fumarate, triallyl isocyanurate, etc. can also be used. These free radical polymerizable monomers can be used alone or in combination of two or more.
[0162] As the radical polymerizable multimer in the present invention, diallyl phthalate prepolymer, TAIC prepolymer, epoxy prepolymer, urethane prepolymer, acrylate prepolymer can be used. These radical polymerizable multimers can be used alone or in combination of two or more.
[0163] In the crystalline free radical polymerizable composition for electrical and electronic parts of the present invention, an inorganic filler can be matched. As for the inorganic filler, calcium carbonate, magnesium carbonate, barium carbonate, calcium hydroxide, aluminum hydroxide, magnesium hydroxide, magnesium oxide, aluminum oxide, silicon dioxide, zinc oxide, mica, talc, aluminum nitride, boron nitride can be listed. Among these, aluminum oxide and magnesium oxide are preferred from the viewpoint of thermal conductivity. These can be used alone or in combination of two or more. According to the present invention, a composition of an inorganic filler that can be used after considering the cost performance can be realized in large quantities, so a higher thermal conductivity can be achieved. In fact, if special and expensive inorganic fillers (aluminum nitride, boron nitride), carbon nanotubes, diamonds, metal powders, etc. are used, it becomes high thermal conductivity and can be used, and has the advantages of good operability and fluidity, but the expensive inorganic fillers of carbon nanotubes, metal powders, etc. are not practical, so aluminum oxide, magnesium oxide, etc. can be used.
[0164] As the above-mentioned inorganic filler, an inorganic filler having an average particle size of less than 150 μm, preferably 0.01 to 80 μm, can be used. By using an inorganic filler having the above-mentioned average particle size, a crystalline free radical polymerizable composition for electrical and electronic parts having excellent fluidity and strength during molding can be made. In addition, the above-mentioned range is set because: the use of an inorganic filler having a large thermal conductivity is likely to be advantageous. In the case of a large amount of inorganic fillers having a small average particle size, the thermal conductivity of the resin is low, so thermal resistance is generated, and there is a concern that the thermal conductivity of the molded product is reduced. Therefore, in the case of using an inorganic filler having a large average particle size, it is advantageous for thermal conduction, but an excessively large inorganic filler has concerns about appearance (surface concave-convex) and inability to fill into a fine part. From such a viewpoint, it can be limited to a certain size.
[0165] The average particle size is measured by laser diffraction, and the JIS standard is JIS Z8825-1. JIS Z8825-1 is abolished in H25.12.20 and replaced by JIS Z8825. JIS Z8825-1 is a particle size analysis-laser diffraction method.
[0166] The crystalline radical polymerizable composition for electric and electronic components of the present invention may be blended with various additives that are closely coupled with the inorganic filler and the reinforcing material, for example, a (meth)acrylate compound having a polar group or a coupling agent.
[0167] The (meth)acrylate compound having a polar group is not particularly limited, and examples thereof include (meth)acrylate compounds having a substituent containing atoms other than carbon and hydrogen and ester-bonded, and examples thereof include hydroxyl, epoxy, glycidyl ether, tetrahydrofuranyl, isocyanate, carboxyl, alkoxysilyl, phosphate, lactone, oxetane, tetrahydropyranyl, amino, etc. The coupling agent is not particularly limited, and examples thereof include silane coupling agents and titanate coupling agents, and examples thereof include epoxy silane, amino silane, cationic silane, vinyl silane, acrylic silane, mercapto silane, and composites thereof.
[0168] Among these, acrylic silane coupling agents are preferred from the viewpoint of improving strength. In addition, various additives may be used as long as the purpose of the present invention is not impaired.
[0169] In the crystalline radical polymerizable composition for electric and electronic parts of the present invention, an organic peroxide generally used in unsaturated polyester resin compositions and radical polymerizable compositions can be used as a radical polymerization initiator or inhibitor.
[0170] Examples of the organic peroxide include tert-butyl peroxy-2-ethylhexyl monocarbonate, 1,1-di(tert-hexylperoxy)cyclohexane, 1,1-di(tert-butylperoxy)cyclohexane, 1,1-di(tert-butylperoxy)-3,3,5-trimethylcyclohexane, tert-butyl peroxyoctanoate, benzoyl peroxide, methyl ethyl ketone peroxide, acetylacetone peroxide, tert-butyl peroxybenzoate, dicumyl peroxide, etc. These may be used alone or in combination of two or more.
[0171] Among these, from the viewpoint of molding conditions and storage stability, it is preferable to use an organic peroxide having a 10-hour half-life temperature of 90° C. or higher, and specifically, it is preferable to use dicumyl peroxide.
[0172] Examples of the polymerization inhibitor include hydroquinone, monomethyl ether hydroquinone, methyl hydroquinone, di-tert-4-methylphenol, monomethyl ether hydroquinone, phenothiazine, tert-butylcatechol, p-benzoquinone, pyrogallol and other quinones, 2,6-di-tert-butyl-p-cresol, 2,2-methylene-bis-(4-methyl-6-tert-butylphenol), 1,1,3-tris-(2-methyl-4-hydroxy-5-tert-butylphenyl)butane and other phenolic compounds, Piperidine-1-oxy free radicals such as 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxy free radical, 4-oxo-2,2,6,6-tetramethylpiperidin-1-oxy free radical, 4-methoxy-2,2,6,6-tetramethylpiperidin-1-oxy free radical, 4-carboxyl-2,2,6,6-tetramethylpiperidin-1-oxy free radical, and 2,2,6,6-tetramethylpiperidin-1-oxy free radical. By using these, thickening during the filling period during molding can be suppressed, and a free radical polymerizable composition with low melt viscosity can be prepared. These can be used alone or in combination of two or more.
[0173] The crystalline radical polymerizable composition for electric and electronic components of the present invention may contain a reinforcing material. By using the reinforcing material, the crystalline radical polymerizable composition for electric and electronic components having excellent strength characteristics and dimensional stability can be obtained.
[0174] As the reinforcing material used in the present invention, glass fiber used in fiber-reinforced plastics such as BMC (bulk molding compound) and SMC (sheet molding compound) can be generally used, but the present invention is not limited to glass fiber and other materials can also be used.
[0175] As glass fibers, there can be mentioned glass fibers such as E glass (alkali-free glass for electrical use), C glass (alkali-containing glass for chemical use), A glass (acid-resistant glass), and S glass (high-strength glass) made of silicate glass and borosilicate glass, and articles made of these into long fibers (rovings), short fibers (chopped strands), and ground fibers can also be used. In addition, articles that have been subjected to surface treatment can also be used for these glass fibers.
[0176] Furthermore, the crystalline radically polymerizable composition for electric and electronic components of the present invention may contain other inorganic fillers as appropriate within a range not impairing the properties of a molded article.
[0177] Examples of these materials include oxides and hydrates thereof, inorganic foamed particles, and hollow particles such as silica balloons.
[0178] Furthermore, a thermoplastic resin may be appropriately blended into the crystalline radically polymerizable composition for electric and electronic components of the present invention within a range that does not inhibit the properties of a molded article.
[0179] Examples of these resins include thermoplastic resins such as polystyrene, acrylic resins, polyvinyl acetate, saturated polyesters, styrene-butadiene rubber, and organic foamed particles.
[0180] In the crystalline free radical polymerizable composition for electrical and electronic parts of the present invention, a release agent can be used. As a release agent, fatty acid series, fatty acid metal salt series, mineral series, etc. waxes used in general thermosetting resins can be used, and fatty acid series, fatty acid metal salt series, and waxes with excellent heat discoloration resistance are particularly preferably used.
[0181] Specific examples of these release agents include stearic acid, zinc stearate, aluminum stearate, calcium stearate, paraffin, etc. These release agents may be used alone or in combination of two or more.
[0182] As the mold release agent, an external mold release agent such as a mold release agent that is sprayed or applied to a mold, or a molding material in which a mold release agent is blended may be used as necessary.
[0183] In the crystalline free radical polymerizable composition for electrical and electronic parts of the present invention, a flame retardant can be used. As the flame retardant, a halogen-based, phosphorus-based, nitrogen-based, composite organic flame retardant, and an inorganic flame retardant of a metal hydroxide, antimony-based, red phosphorus-based, silicone-based, or borate can be used. In addition, as for these flame retardants, an additive flame retardant or a reactive flame retardant that reacts with the resin and enters the resin skeleton can be used. These flame retardants can be used alone or in combination of two or more.
[0184] In the present invention, in addition to these ingredients, a curing catalyst, polymerization inhibitor, colorant, thickener, wetting and dispersing agent, surface conditioner, viscosity reducer, flow modifier, other organic additives, inorganic additives, etc. for adjusting the curing conditions of the crystalline free radical polymerizable composition may be appropriately formulated as needed.
[0185] <Method for producing crystalline radical polymerizable composition>
[0186] The crystalline radical polymerizable composition for electric and electronic parts of the present invention can be produced by blending the components using a stirrer, blender or the like, mixing them sufficiently and uniformly, and then preparing and granulating them using a kneading machine, extruder or the like capable of heating and pressurizing.
[0187] Furthermore, the granular material of the present invention is characterized by comprising the crystalline radically polymerizable composition for electric and electronic components of the present invention.
[0188] The electric and electronic component molded body of the present invention is characterized by molding a granular material containing the crystalline radical polymerizable composition for electric and electronic components of the present invention. The electric and electronic component molded body can be molded by various molding methods of thermosetting compositions according to conventional methods.
[0189] In addition, the crystalline free radical polymerizable composition for electrical and electronic parts of the present invention is dry and has good thermal stability when melted, so it is preferably used as a molding method. Injection molding, injection compression molding, transfer molding, compression molding, or melt heating molding such as hot melt molding.
[0190] Among these, injection molding using an injection molding machine and transfer molding using a transfer molding machine are particularly preferred. The injection molding method can shorten the molding time, and the transfer molding method can mold multiple molded bodies at a time, so that complex-shaped electrical and electronic parts molded bodies can be produced.
[0191] <Electrical and electronic component molded body and method for producing the same>
[0192] The electric and electronic component molded body of the present invention can be produced by molding the electric and electronic component molded body using the crystalline radical polymerizable composition for electric and electronic components of the present invention. Here, the crystalline radical polymerizable composition for electric and electronic components of the present invention may be a composition in which all components constituting the crystalline radical polymerizable composition are separately pre-heated and kneaded, or a composition in which a part or all of the components are mixed and heated and kneaded just before being injected into a mold.
[0193] The temperature and pressure of the crystalline free radical polymerizable composition during mold injection are not particularly limited. When an injection molding machine is used, the temperature of the crystalline free radical polymerizable composition is 60 to 130° C., the mold temperature is 130 to 190° C., and the pressure of the crystalline free radical polymerizable composition is 0.1 to 10 MPa. In the case of a transfer molding machine, if the mold temperature is 130 to 190° C. and the pressure of the crystalline free radical polymerizable composition is 0.1 to 10 MPa, damage to electrical and electronic parts is reduced, which is preferred.
[0194] Example
[0195] Hereinafter, one embodiment of the present invention will be described in further detail with reference to examples, but the present invention is not limited to these examples at all.
[0196] <Production Example of Radically Polymerizable Composition for Sealing Electrical and Electronic Components>
[0197] Examples 1 to 11, Reference Example 1, and Comparative Examples 1 to 2
[0198] The crystalline or amorphous radical polymerizable compositions of Examples 1 to 11 shown in Table 2, Reference Example 1, and Comparative Examples 1 to 2 shown in Table 3 were blended in accordance with the blending amounts described in Tables 2 and 3 below, and uniformly mixed using a kneading machine capable of pressurized heating and cooling, and then fed into an extruder and hot cut to form pellets. Some of the pellets and block-like radical polymerizable compositions were powdered using a pulverizer.
[0199] The obtained radical polymerizable composition was used to prepare a test piece by a hydraulic molding machine (manufactured by Toho Press Manufacturing Co., Ltd.) at a mold temperature of 165°C and a curing time of 180 seconds or a curing time until a test piece can be obtained. The physical properties of the molded test piece were evaluated by the following methods, which are shown in Tables 2 and 3, respectively.
[0200] The following components were used as compounding components.
[0201] (1) Polymerizable compounds
[0202] 1. Crystalline free radical polymerizable compound 1: Phthalic acid-based unsaturated polyester (condensation product of terephthalic acid, fumaric acid and 1,6-hexanediol)
[0203] 2. Crystalline free radical polymerizable compound 2: Urethane methacrylate (2-hydroxyethyl methacrylate adduct of 1,6-hexamethylene diisocyanate)
[0204] 3. Crystalline free radical polymerizable compound 3: Urethane acrylate (2-hydroxyethyl acrylate adduct of 1,6-hexamethylene diisocyanate)
[0205] 4. Crystalline free radical polymerizable monomer 1: Ethoxylated isocyanuric acid triacrylate (A-9300 manufactured by Shin-Nakamura Chemical Co., Ltd.)
[0206] 5. Amorphous free radical polymerizable compound 1: Phthalic acid-based unsaturated polyester (U-PICA 8552H manufactured by U-PICA Co., Ltd., Japan)
[0207] 6. Amorphous free radical polymerizable compound 2: Bisphenol A epoxy methacrylate (methacrylic acid adduct of bisphenol A epoxy resin)
[0208] 7. Radical polymerizable monomer 1: diallyl phthalate monomer (DAISO DAP monomer manufactured by Osaka SODA Co., Ltd.)
[0209] 8. Radical polymerizable monomer 2: diethylene glycol dimethacrylate (2G manufactured by Shin-Nakamura Chemical Co., Ltd.)
[0210] (2) Inorganic filling materials
[0211] 1. Inorganic filler 1: fused silica (manufactured by Denka Corporation, average particle size 24 μm)
[0212] 2. Inorganic filler 2: calcium carbonate (manufactured by Nitto Powder Chemical Co., Ltd., average particle size 2 μm)
[0213] (3) Additives
[0214] 1. Silane coupling agent: methacrylic silane (KBM-503 manufactured by Shin-Etsu Chemical Co., Ltd.)
[0215] 2. Radical polymerization initiator: dicumyl peroxide (PERCUMYL D manufactured by NOF Corporation)
[0216] 3. Release agent: zinc stearate (GF-200 manufactured by NOF Corporation)
[0217] 4. Inhibitor: p-Benzoquinone (PBQ manufactured by Seiko Chemical Co., Ltd.)
[0218] 5. Colorant: Carbon black (CB40 manufactured by Mitsubishi Chemical Corporation)
[0219] <Polymerizable Compound Characteristics>
[0220] The melting points and weight average molecular weights of the crystalline or amorphous radical polymerizable compound and the radical polymerizable monomer were measured and are shown in Table 1.
[0221] Table 1
[0222] Melting point [℃] Weight average molecular weight Crystalline free radical polymerizable compound 1 Phthalic acid unsaturated polyester 83 11400 Crystalline free radical polymerizable compound 2 Urethane Methacrylate 77 800 Crystalline free radical polymerizable compound 3 Urethane Acrylate 75 800 Crystalline free radical polymerizable monomer 1 Ethoxylated isocyanurate triacrylate 55 600 Amorphous free radical polymerizable compound 1 Phthalic acid unsaturated polyester - 41700 Amorphous free radical polymerizable compound 2 Bisphenol A epoxy acrylate - 3000 Free radical polymerizable monomer 1 Diallyl Phthalate Monomer - 400 Free radical polymerizable monomer 2 Diethylene glycol dimethacrylate - 400
[0223]
[0224] Table 3
[0225] unit Comparative Example 1 Comparative Example 2 Amorphous free radical polymerizable compound 1 Phthalic acid unsaturated polyester weight% 70 Amorphous free radical polymerizable compound 2 Bisphenol A epoxy methacrylate weight% 100 Free radical polymerizable monomer 1 Diallyl Phthalate Monomer weight% 30 Inorganic filling materials 1 Fused Silica weight% 650 650 Inorganic filling materials 2 Calcium phosphate weight% Silane coupling agent Methacrylate silane weight% 3 3 Free Radical Polymerization Initiator Dicumyl peroxide weight% 1 1 Release agent Zinc stearate weight% 10 10 Inhibitor p-Benzoquinone weight% 0.1 0.1 Colorants Carbon Black weight% 0.2 0.2 total 764 764 hardness 5 60 Melt viscosity Pa·s 500 3000 Flow length cm 40 60 Molding shrinkage % 0.2 0.3 Glass transition temperature ℃ 200 130
[0226] <Compound Characteristics, Composition Characteristics, and Physical Property Evaluation Methods>
[0227] (1) Melting point
[0228] Using a differential scanning calorimeter "DSC6220" (manufactured by Seiko Instruments Co., Ltd.), 10 mg of the free radical polymerizable compound test sample shown in Table 1 was placed in an aluminum pan, covered and sealed, and measured from -60°C to 200°C at a heating rate of 10°C / min. The endothermic peak of the obtained curve was taken as the melting point. The results are shown in Table 1. The measurement was terminated for compounds that were liquid at 23°C.
[0229] (2) Weight average molecular weight
[0230] The weight average molecular weight of the free radical polymerizable compound shown in Table 1 is measured by dissolving the polymerizable compound in tetrahydrofuran (THF) at 1.0 wt %, and using GPC (gel permeation chromatography) in terms of polystyrene. The measurement conditions are shown below. The results are shown in Table 1. However, even if the above strict criteria are not met, depending on the desired use, the required quality, etc., sometimes a weight average molecular weight of less than 100 or greater than 100,000 is also suitable, so it is only necessary to study it as an indicator.
[0231] Instrument: Shodex GPC-101 manufactured by Showa Denko K.K.
[0232] Column: KF-802, 803, 804, 805 manufactured by Showa Denko K.K.
[0233] Solvent, carrier liquid: THF
[0234] Flow rate: 1.0ml / min
[0235] Sample concentration: 1.0%
[0236] Temperature: 40℃
[0237] Sample injection volume: 200 μl
[0238] Detector: Differential refractive index detector
[0239] (3) Hardness
[0240] The measurement method is based on JIS K7215. The hardness of the crystalline or amorphous radical polymerizable composition of Examples 1 to 11 shown in Table 2, Reference Example 1 and Comparative Examples 1 to 2 shown in Table 3 was measured with a hardness meter (WR-105D, Nishi-Tokyo Precision Co., Ltd.). The radical polymerizable composition adjusted to 90°C was formed into a flat plate of about 100 mm × 100 mm × 10 mm, and cooled and solidified in a constant temperature room at 23°C. The radical polymerizable composition before curing adjusted to 23°C was placed on a horizontal hard table. The pressurizing reference surface of the hardness meter was kept parallel to the surface of the radical polymerizable composition, and pressed as quickly as possible on the surface of the radical polymerizable composition without impact, so that the pressurizing reference surface and the radical polymerizable composition were fully in close contact. The maximum indication value of the pointer of the indicator device was quickly read within 1 second. The results are shown in Tables 2 and 3. The target hardness is 10, 20 or more is excellent, 10 or more is good, and less than 10 is acceptable.
[0241] (4) Melt viscosity
[0242] The melt viscosity of the crystalline or amorphous radical polymerizable compositions of Examples 1 to 11 shown in Table 2, Reference Example 1, and Comparative Examples 1 to 2 shown in Table 3 was measured using a high-flow flow tester (CFT-100EX manufactured by Shimadzu Corporation). The radical polymerizable composition was placed in a sample insertion hole of a cylinder having a die head of 0.5 mm in diameter and 1 mm in length and heated to 90°C, and after preheating for 240 seconds, the mixture was heated at 30 kgf / cm 2 or 1kgf / cm 2 The piston was pressurized with a pressure of 1.50 and the radical polymerizable composition was made to flow out from the nozzle of the die head, and the melt viscosity was determined from the point where the linearity was good. The results are shown in Tables 2 and 3. The target melt viscosity was 1 to 1000 Pa·s, and the composition with 1 to 100 Pa·s was excellent, and 100 to 1000 Pa·s was good.
[0243] (5) Flow length
[0244] The measurement method is based on EIMS T-901. Using the crystalline or amorphous radical polymerizable compositions of Examples 1 to 11 shown in Table 2, Reference Example 1, and Comparative Examples 1 to 2 shown in Table 3, the flow length is measured using an auxiliary piston transfer molding machine equipped with a spiral flow mold. The spiral flow mold is heated to 165°C. The spiral flow mold uses a mold with a central portion as the injection port of the material, and a semicircular groove with a radius of 1.6 mm is set in a spiral curve shape starting from the injection port. A predetermined amount of radical polymerizable composition is measured and the thickness of the residual resin is in the range of 1 to 10 mm. The plunger is pulled up, and the radical polymerizable composition is added to the material port, and a pressure of 3.2 MPa is immediately applied to start transfer molding. The action of the plunger is stopped, and the mold is opened 180 seconds after the start of the measurement, and the molded product is taken out. The length to the glossy part at the front end of the molded product, or the length of the glossy part plus 1 / 2 of the length of the low-density part in front of it is read. The results are shown in Tables 2 and 3. The target flow length is 50 cm, 100 cm or more is excellent, 50 cm or more is good, and less than 50 cm is acceptable. However, even if the above strict standards are not met, depending on the desired use, required quality, etc., sometimes less than 50 cm is also suitable, so it can be studied as an indicator.
[0245] (6) Molding shrinkage
[0246] The measurement method is in accordance with JIS K6911. Using the crystalline or amorphous radical polymerizable compositions of Examples 1 to 11 shown in Table 2, Reference Example 1, and Comparative Examples 1 to 2 shown in Table 3, and using a mold for shrinkage measurement, a test piece was made by compression molding. The radical polymerizable composition was placed in a mold adjusted to 165°C and heated under pressure for 3 minutes. The test piece was immediately taken out of the mold and stored at a constant temperature and humidity of 23°C and 55% RH for 24 hours. Along the measurement lines perpendicular to the outer diameter of the annular belt protruding from the front and back of the test piece, the dimensions of 2 places on the surface and 2 places on the back, a total of 4 places, were measured. The outer diameter of the groove of the mold corresponding to the test piece was measured to 0.01 mm under the same conditions, and the molding shrinkage was calculated. The results are shown in Tables 2 and 3. The target molding shrinkage is set to 0.5%, 0.2% or less is excellent, 0.2 to 0.5% or less is good, and more than 0.5% is acceptable. However, even if the above strict standards are not met, depending on the desired application, required quality, etc., conditions exceeding 0.5% may be suitable, so it can be studied as an indicator.
[0247] (7) Glass transition temperature
[0248] The measurement is based on JIS K7224-4. The crystalline or amorphous free radical polymerizable composition of Examples 1 to 11 shown in Table 2, Reference Example 1 and Comparative Examples 1 to 2 shown in Table 3 are placed in a flat plate mold adjusted to 165°C. The mold is quickly closed and pressurized and heated to form. After curing, the mold is opened to obtain a flat plate-shaped molded piece. The flat plate-shaped molded piece is cut into strips to obtain a test piece for measuring the glass transition temperature. The dynamic viscoelasticity (RSA-G2 manufactured by TA Instruments) is measured at a heating rate of 2°C / min in the range of 30 to 250°C at a frequency of 10 Hz. The Tanδ peak temperature is taken as the glass transition temperature. The results are shown in Tables 2 and 3. The target glass transition temperature is 125°C, and those above 125°C are considered good, and those below 125°C are considered acceptable. However, even if the above strict standards are not met, a temperature of less than 125°C may be suitable under certain conditions depending on the desired application, required quality, etc., so it can be studied as an indicator.
[0249] <Evaluation Results>
[0250] As shown in Table 2 and Table 3, it is found that the crystalline radical polymerizable composition for sealing electrical and electronic parts of the present invention has excellent workability. In addition, in particular, Examples 1 to 8 and 11 of the crystalline radical polymerizable composition for sealing electrical and electronic parts of the present invention are solid at 23°C, and therefore have excellent workability and low melt viscosity, which is good. It is found that the crystalline radical polymerizable composition for sealing electrical and electronic parts of the present invention shows excellent results overall.
[0251] Example 9 is a crystalline radical polymerizable composition with a different inorganic filler content in Example 1. The composition has a hardness of 3 and is soft. In addition, the melt viscosity is 0.5 Pa·s, which is a low viscosity composition. The molding shrinkage is large, but other properties are good.
[0252] Example 10 is a crystalline radical polymerizable composition in which the crystalline radical polymerizable compound of Example 5 is changed to a radical polymerizable compound that is liquid at room temperature, and the mixing ratio of the radical polymerizable compound is changed. Since the amount of the crystalline radical polymerizable compound is small, the hardness of the composition is 0, and it is soft. In addition, the glass transition temperature is low, but other properties are good.
[0253] Reference Example 1 is a crystalline radical polymerizable composition in which the amount of inorganic filler in Example 8 is changed. The melting start temperature was not observed because the flow stopped during the measurement. In addition, the melt viscosity was high and the flow length was also short, but other properties were good.
[0254] Therefore, even in Examples 9 and 10 and Reference Example 1, the conditions may sometimes be suitable depending on the desired application, required quality, etc., so it is sufficient to study them as an indicator to determine that they are applicable to applications requiring good properties.
[0255] In addition, both Comparative Examples 1 and 2 obtained results of high melt viscosity (Comparative Example 1 can be compared with Example 4) and poor operability compared with crystallinity.
[0256] As described above, it was found that the crystalline radically polymerizable composition for sealing electric and electronic components, which contains at least a crystalline radically polymerizable compound, has excellent workability and good fluidity.
[0257] In addition, one embodiment of the crystalline radically polymerizable composition for electric and electronic components of the present invention will be described in further detail below with reference to Examples, but the present invention is not limited to these Examples at all.
[0258] <Production Example of Radically Polymerizable Composition for Electric and Electronic Components>
[0259] Examples 12 to 19 and Comparative Examples 3 to 5
[0260] The crystalline or amorphous radical polymerizable compositions of Examples 12 to 19 and Comparative Examples 3 to 5 shown in Table 4 were blended according to the described blending amounts, and uniformly mixed using a kneading machine capable of pressurized heating and cooling, and then fed into an extruder to form pellets by a hot cut method. Some of the pellets and block-like radical polymerizable compositions were powdered using a pulverizer.
[0261] The obtained radical polymerizable composition was used to prepare a test piece by a hydraulic molding machine (manufactured by Toho Press Manufacturing Co., Ltd.) at a mold temperature of 165°C and a curing time of 180 seconds or a curing time until a test piece can be obtained. The physical properties of the molded test piece (molded body) were evaluated according to the following method, and the results are shown in Tables 4 and 5.
[0262] The following components were used as compounding components.
[0263] (1) Radical polymerizable compounds
[0264] 1. Crystalline free radical polymerizable compound 1: Phthalic acid-based unsaturated polyester (condensation product of terephthalic acid, fumaric acid and 1,3-propylene glycol)
[0265] 2. Crystalline free radical polymerizable compound 2: Urethane methacrylate (2-hydroxyethyl methacrylate adduct of 1,6-hexamethylene diisocyanate)
[0266] 3. Amorphous free radical polymerizable compound 1: Phthalic acid-based unsaturated polyester (U-PICA 8552H manufactured by U-PICA Co., Ltd., Japan)
[0267] 4. Amorphous free radical polymerizable compound 2: Bisphenol A epoxy methacrylate (methacrylic acid adduct of bisphenol A epoxy resin)
[0268] (2) Free radical polymerizable monomers
[0269] 5. Free radical polymerizable monomer 1: Styrene monomer
[0270] 6. Radical polymerizable monomer 2: ethoxylated isocyanuric acid triacrylate (A-9300 manufactured by Shin-Nakamura Chemical Co., Ltd.)
[0271] (3) Inorganic filling materials
[0272] 1. Inorganic filler 1: Alumina (manufactured by Denka Corporation, average particle size 45 μm)
[0273] 2. Inorganic filler 2: magnesium oxide (Ube Materials Co., Ltd., average particle size 55 μm)
[0274] 3. Inorganic filler 3: fused silica (manufactured by Denka Corporation, average particle size 24 μm)
[0275] (4) Additives
[0276] 1. Silane coupling agent: methacrylic silane (KBM-503 manufactured by Shin-Etsu Chemical Co., Ltd.)
[0277] 2. Radical polymerization initiator: dicumyl peroxide (PERCUMYLD manufactured by NOF Corporation)
[0278] 3. Release agent: zinc stearate (GF-200 manufactured by NOF Corporation)
[0279] 4. Thermoplastic resin: Polystyrene (G-100C manufactured by Toyo Polystyrene Co., Ltd.)
[0280] 5. Inhibitor: p-Benzoquinone (PBQ manufactured by Seiko Chemical Co., Ltd.)
[0281] 6. Colorant: Carbon black (CB40 manufactured by Mitsubishi Chemical Corporation)
[0282]
[0283] Table 5
[0284] Comparative Example 3 Comparative Example 4 Comparative Example 5 Crystalline free radical polymerizable compound 1 Crystalline free radical polymerizable compound 2 Amorphous free radical polymerizable compound 1 50 60 Amorphous free radical polymerizable compound 2 50 Free radical polymerizable monomer 1 50 40 50 Free radical polymerizable monomer 2 Inorganic filling materials 1 1000 1000 Inorganic filling materials 2 100 Inorganic filling materials 3 Coupling agent 2 2 2 Release agent 14 14 14 Colorants 8 8 8 Thermoplastic resin 30 30 Polymerization initiator 3 3 3 Inhibitor 0.1 0.1 0.1 Melting point [℃] - - - Weight average molecular weight 41700 41700 3000 hardness [-] 5 7 5 Thermal conductivity [W / m·K] 4.7 0.4 4.7 Melt viscosity [Pa·s] 800 1000 500
[0285] <Compound Characteristics, Composition Characteristics, and Physical Property Evaluation Methods>
[0286] (1) Melting point
[0287] Using a differential scanning calorimeter "DSC6220" (manufactured by Seiko Instruments), 10 mg of the free radical polymerizable compound test sample shown in Table 4 and Table 5 was placed in an aluminum pan, covered and sealed, and measured from -60°C to 200°C at a heating rate of 10°C / min. The endothermic peak of the obtained curve was taken as the melting point. The results are shown in Table 4 and Table 5. The measurement was terminated for compounds that were liquid at 23°C.
[0288] (2) Weight average molecular weight
[0289] The weight average molecular weight of the radical polymerizable compounds shown in Tables 4 and 5 is measured by dissolving the radical polymerizable compounds in tetrahydrofuran (THF) at 1.0 wt %, and using GPC (gel permeation chromatography) to convert the free radical polymerizable compounds to polystyrene. In the case of two radical polymerizable compounds, the molecular weight of the larger one is recorded. The results are shown in Tables 4 and 5. However, even if the above strict criteria are not met, there are also suitable cases where the weight average molecular weight is less than 70 or greater than 100,000 according to the desired use, the required quality, etc., so it is sufficient to study it as an indicator.
[0290] Instrument: Shodex GPC-101 manufactured by Showa Denko K.K.
[0291] Column: KF-802, 803, 804, 805 manufactured by Showa Denko K.K.
[0292] Solvent, carrier liquid: THF
[0293] Flow rate: 1.0ml / min
[0294] Sample concentration: 1.0%
[0295] Temperature: 40℃
[0296] Sample injection volume: 200 μl
[0297] Detector: Differential refractive index detector
[0298] (2) Hardness
[0299] The measurement method is based on JIS K7215. Using a hardness tester (WR-105D, Nishi-Tokyo Precision Co., Ltd.), the hardness of the crystalline or amorphous radical polymerizable composition of Examples 12 to 19 and Comparative Examples 3 to 5 shown in Tables 4 and 5 was measured. The radical polymerizable composition adjusted to 90°C was formed into a flat plate of about 100 mm × 100 mm × 10 mm, and cooled and solidified in a constant temperature room at 23°C. The radical polymerizable composition before curing adjusted to 23°C was placed on a horizontal hard table. The pressurization reference surface of the hardness tester was kept parallel to the surface of the radical polymerizable composition, and at the same time, it was pressed as quickly as possible without impact, so that the pressurization reference surface and the radical polymerizable composition were fully in close contact. The maximum indication value of the pointer of the indicator device was quickly read within 1 second. The results are shown in Tables 4 and 5. The target hardness is set to 10, 15 or more is excellent, 10 or more is good, and less than 10 is acceptable. However, even if the above strict standards are not met, conditions less than 10 may be appropriate depending on the desired application, required quality, etc., so it can be studied as an indicator.
[0300] (3) Thermal conductivity
[0301] The measurement method is ISO22007-2. The thermal conductivity is measured using the molded bodies of the crystalline or amorphous free radical polymerizable compositions of Examples 12 to 19 and Comparative Examples 3 to 5 shown in Tables 4 and 5. The molded body of the free radical polymerizable resin composition was cut into 100 mm square and 3 mm thick, and measured at 23°C by the hot plate method (thermal conductivity measuring device TPS2500S manufactured by Kyoto Electronics Industry Co., Ltd.). The results are shown in Tables 4 and 5. The target thermal conductivity is set to 1.0 W / m·K, 1.5 W / m·K and above is set as excellent, 1.0 W / m·K and above is set as good, and less than 1.0 W / m·K is set as acceptable. However, even if the above strict standards are not met, depending on the desired application, the required quality, etc., the condition of less than 1.0 W / m·K is sometimes suitable, so it can be studied as an indicator.
[0302] (4) Melt viscosity
[0303] The crystalline or amorphous radical polymerizable compositions of Examples 12 to 19 and Comparative Examples 3 to 5 shown in Tables 4 and 5 were measured for melt viscosity using a high-speed flow tester (CFT-100EX manufactured by Shimadzu Corporation). The radical polymerizable composition was placed in a sample insertion hole of a cylinder having a die head of 2.0 mm in diameter and 10 mm in length and heated to 90°C, and after preheating for 240 seconds, the melt viscosity was measured at 3 to 100 kgf / cm 2 The piston is pressurized with a pressure of 1000 s to make the free radical polymerizable composition flow out from the nozzle of the die head. The melt viscosity of the composition is determined from the place where the linearity is good. The melt viscosity of the composition is measured at more than 3 points, and the relationship between the melt viscosity and the shear rate of the composition is studied. From the relationship between the melt viscosity and the shear rate of the composition, the shear rate is determined by interpolation or extrapolation to be 1000 s -1 The melt viscosity is shown in Tables 4 and 5. The target viscosity is set at 10 to 2,000 Pa·s, and compositions of 10 to 1,000 Pa·s are considered excellent, 1,000 to 2,000 Pa·s are considered good, and less than 10 Pa·s and / or 2,000 Pa·s are considered acceptable. However, even if the above strict standards are not met, depending on the desired use and the required quality, less than 10 Pa·s and / or more than 2,000 Pa·s may be suitable, so it is sufficient to study it as an indicator.
[0304] <Evaluation Results>
[0305] As shown in Table 4, Examples 12 to 19 of the crystalline radically polymerizable composition for electric and electronic components of the present invention were found to be solid at 23° C. and thus to be excellent in handleability.
[0306] In addition, Comparative Example 3 is a material in which the crystalline radical polymerizable compound 1 of Example 12 is replaced by the amorphous radical polymerizable compound 1, and the mixing ratio of the inorganic filler is changed. In Comparative Example 4, the crystalline radical polymerizable compound 1 of Example 14 is replaced by the amorphous radical polymerizable compound 1. In addition, Comparative Example 5 is a material in which the crystalline radical polymerizable compound 1 of Example 12 is replaced by the amorphous radical polymerizable compound 2, and the mixing ratio of the inorganic filler is changed. As a result, the composition using only the amorphous radical polymerizable compound is poor in usability.
[0307] As described above, it was found that the crystalline radically polymerizable composition for electric and electronic components containing at least a crystalline radically polymerizable compound is excellent in thermal conductivity and handleability.
[0308] Industrial Applicability
[0309] The crystalline radical polymerizable composition for sealing electric and electronic parts of the present invention and the electric and electronic parts sealed body formed using the same have a high glass transition temperature and excellent heat resistance, and thus can improve the durability of various connectors, wiring harnesses, semiconductor sealed bodies or electronic parts sealed bodies for automobiles, communications, computers, and home appliances, switches with printed circuit boards, sensors, and other electric and electronic parts, electric and electronic parts sealed bodies, and the like.
[0310] In addition, the crystalline radical polymerizable composition for electric and electronic parts of the present invention and the electric and electronic parts molded bodies formed using the same have excellent thermal conductivity, and thus can improve the durability of various connectors, coils, semiconductor sealed bodies or electronic parts sealed bodies for automobiles, communications, computers, and home appliances, switches with printed circuit boards, sensors, and other electric and electronic parts, electric and electronic parts molded bodies, and the like.
Claims
1. A crystalline free radical polymerizable composition for sealing electrical and electronic parts, It is characterized in that The composition contains at least a crystalline radical polymerizable compound, an inorganic filler, a silane coupling agent, and a radical polymerization initiator.
2. The crystalline radical polymerizable composition for sealing electric and electronic parts according to claim 1, in, The crystalline radical polymerizable compound includes one or more selected from unsaturated polyesters, epoxy (meth)acrylates, urethane (meth)acrylates, polyester (meth)acrylates, polyether (meth)acrylates, radical polymerizable monomers, and radical polymerizable multimers.
3. The crystalline radical polymerizable composition for sealing electric and electronic parts according to claim 1 or 2, in, The melting point of the crystalline radical polymerizable compound is in the range of 30 to 150°C.
4. The crystalline radical polymerizable composition for sealing electric and electronic components according to any one of claims 1 to 3, in, The crystalline radical polymerizable composition is solid at 23°C.
5. The crystalline radical polymerizable composition for sealing electric and electronic components according to any one of claims 1 to 4, in, The melt viscosity of the crystalline radical polymerizable composition measured by a high-flow tester was measured at a temperature of 90° C., a die diameter of 0.5 mm, a length of 1.0 mm, and a pressure of 30 kgf / cm 2 7~1000Pa·s, or at a pressure of 1kgf / cm 2 It is 1~7Pa·s.
6. The crystalline radical polymerizable composition for sealing electric and electronic components according to any one of claims 1 to 5, in, The inorganic filler is present in an amount of 50 to 95% by weight based on the total amount of the crystalline radical polymerizable composition.
7. The crystalline radical polymerizable composition for sealing electric and electronic components according to any one of claims 1 to 6, in, The ratio of the crystalline radically polymerizable compound to the total amount of the radically polymerizable compounds is 30 parts by weight or more.
8. The crystalline radical polymerizable composition for sealing electric and electronic components according to any one of claims 1 to 7, in, The weight average molecular weight of the crystalline radical polymerizable compound is 100 to 100,000. 9 . A sealed electric and electronic component, which is sealed with the crystalline radically polymerizable composition for sealing an electric and electronic component according to claim 1 . 10 . A granular material comprising the crystalline radically polymerizable composition for sealing electric and electronic components according to claim 1 .
11. A method for producing a sealed electric and electronic component, comprising: sealing an electric and electronic component by insert molding using injection molding or transfer molding of the granular material comprising the crystalline radical polymerizable composition for sealing an electric and electronic component according to claim 10.
12. A crystalline free radical polymerizable composition for electrical and electronic parts, It is characterized in that The composition contains at least a crystalline radical polymerizable compound, an inorganic filler, a silane coupling agent, and a radical polymerization initiator.
13. The crystalline radical polymerizable composition for electric and electronic components according to claim 12, in, The thermal conductivity of a molded body obtained by molding the crystalline radically polymerizable composition for an electric or electronic component is 1.0 W / m·K or more.
14. The crystalline radical polymerizable composition for electric and electronic components according to claim 12 or 13, in, The crystalline radical polymerizable compound includes one or more selected from unsaturated polyesters, epoxy (meth)acrylates, urethane (meth)acrylates, polyester (meth)acrylates, polyether (meth)acrylates, radical polymerizable monomers, and radical polymerizable multimers.
15. The crystalline radical polymerizable composition for electric and electronic components according to any one of claims 12 to 14, in, The melting point of the crystalline radical polymerizable compound is in the range of 30 to 150°C.
16. The crystalline radical polymerizable composition for electric and electronic components according to any one of claims 12 to 15, in, The crystalline radical polymerizable composition is solid at 23°C.
17. The crystalline radical polymerizable composition for electric and electronic components according to any one of claims 12 to 16, in, The inorganic filler is contained in an amount of 40 to 95% by weight based on the total amount of the crystalline radical polymerizable composition.
18. The crystalline radical polymerizable composition for electric and electronic components according to any one of claims 12 to 17, in, The ratio of the crystalline radically polymerizable compound to the total amount of the radically polymerizable compound is 25 parts by weight or more.
19. The crystalline radical polymerizable composition for electric and electronic components according to any one of claims 12 to 18, in, The crystalline radical polymerizable compound has a weight average molecular weight of 70 to 100,000. 20 . An electric and electronic component molded product molded from the crystalline radically polymerizable composition for an electric and electronic component according to claim 12 .
21. The electric and electronic component molded body according to claim 20, in, The thermal conductivity of the molded body is 1.0 W / m·K or more.
22. A granular material comprising the crystalline radically polymerizable composition for electric and electronic components according to any one of claims 12 to 19.
23. A method for manufacturing an electrical and electronic component molded body, comprising: a molding step of molding the granular material containing the crystalline free radical polymerizable composition for electrical and electronic components described in claim 22 into an electrical and electronic component molded body by any method selected from the group consisting of injection molding, transfer molding, compression molding, and hot melt molding.