Preparation method of iridium sputtering target material with low loss rate and iridium sputtering target material
By using vacuum high-frequency induction heating furnace and electromagnetic stirring technology in the preparation of iridium sputtering targets, combined with directional solidification and atmosphere heat treatment, the problem of high loss rate of iridium metal is solved, and low loss rate and low cost iridium sputtering is achieved Target production.
Patent Information
- Application Number
- CN202410911398.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-09
AI Technical Summary
The loss rate of iridium metal in the existing iridium sputtering target preparation process is high, resulting in high production costs and waste of resources.
Iridium sheet smelting is performed by vacuum high-frequency induction heating furnace, combined with electromagnetic stirring and directional solidification technology, protecting protective gases to avoid oxidation, and use an atmosphere heat treatment furnace and protective gas to cover it during the rolling process to control the finished product of iridium targets. The thickness of the reaction layer reduces the loss rate.
The low loss rate of iridium sputtering target is achieved, which reduces production costs, and ensures the performance of iridium sputtering target. The loss rate is less than 1‰ and the cost is reduced by 10-20%.
Smart Images

Figure CN118957509A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of precious metal sputtering target materials, and in particular relates to a method for preparing an iridium sputtering target material with a low loss rate and the iridium sputtering target material. Background Art
[0002] Iridium (Ir) is a platinum group metal with a face-centered cubic structure. Its melting point is as high as 2443°C, which is the highest melting point of any precious metal. It has a high density (22.65 g / cm 3 ), stable chemical properties, high hardness, good high temperature performance, is one of the metals with the best thermal strength and thermal stability at high temperatures, and also a metal with a very high melting point and strong oxidation resistance. In addition, it is also one of the most corrosion-resistant metals, able to withstand the erosion of many molten reagents and high-temperature silicates. It can resist the corrosion of almost all acids, aqua regia, molten metals, and even silicates at high temperatures.
[0003] Due to its excellent physical and chemical stability, iridium thin films are increasingly used in the electronic information industry. For example, in micro-electromechanical systems (MEMS), pure iridium thin films are used as upper electrode layers (for lead-out electrodes) and lower electrode layers (for connecting substrate layers), and Ir-Ta-O composite thin films are used as electrode layers of ferroelectric capacitors in integrated circuits. Pure iridium thin films are directly obtained by magnetron sputtering in an argon atmosphere using iridium sputtering targets as source materials, while Ir-Ta-O composite thin films are obtained by reactive co-sputtering using iridium targets and tantalum targets in an oxygen atmosphere.
[0004] Iridium sputtering target is the raw material for preparing iridium film. Iridium sputtering target is made of iridium metal. Iridium metal has a high melting point, and the loss of traditional process is high, because after smelting, oxidized slag will be produced on the surface of the ingot. After hot rolling, the oxidized slag will expand and fall off under the action of stress and strain, which will cause the loss rate of iridium metal to be lost, often higher than 2‰. High loss not only makes the production cost of iridium sputtering target high, but also leads to the problem of waste of resources. Summary of the invention
[0005] In view of the problems existing in the prior art, the present invention improves the preparation process of iridium sputtering target from the perspective of reducing the production cost of iridium sputtering target, so that the loss rate of iridium in the preparation process of iridium target is less than 1‰, while ensuring the performance of iridium sputtering target. The present invention provides a method for preparing iridium sputtering target with low loss rate and iridium sputtering target, which specifically includes the following contents:
[0006] A method for preparing an iridium sputtering target with a low loss rate comprises the following steps:
[0007] (1) Melting: Add iridium sheets with a purity of not less than 4N into a vacuum high-frequency induction heating furnace. Spread the iridium sheets tightly along the melting crucible and evacuate the furnace to 9×10-4 Pa-9×10 -3 Pa, and then fill with protective gas to a vacuum degree of 7×10 4 Pa-9×10 4 Pa, smelting at a temperature of 2500-2700℃ to obtain iridium melt; compared with the vacuum medium frequency induction heating furnace used in the prior art, this patent uses a vacuum high frequency induction heating furnace to melt iridium sheets. The vacuum high frequency induction heating furnace has the advantages of low cost, small footprint, fast heating rate, and small single melting feed amount. Before the smelting starts, the gas in the cavity is extracted and filled with protective gas to maintain 7×10 4 Pa-9×10 4 The vacuum degree of Pa can effectively prevent the melt from being oxidized by direct contact with air and reduce the burn-in of the melt.
[0008] (2) Refining: The iridium melt is continuously heated in a vacuum high-frequency induction heating furnace, the melt temperature is maintained at 2600-2700°C, and electromagnetic stirring is turned on; the method described in the present invention strictly controls the range of the melt temperature, and can reduce oxidation while ensuring sufficient melting, thereby reducing the loss of raw materials.
[0009] (3) Directional solidification: Use a water-cooled mold with cooling water at the bottom to cast the iridium melt. The casting process is as follows: first, 5-8 cm 3 / s to 1 / 5-1 / 3 of the water-cooled mold; then slow down the casting speed to 3-5cm 3 / s, casting to 2 / 5-3 / 5 of the water-cooled mold; then 1-2cm 3 / s slowly casting, after the casting is completed and cooled, get the ingot; when the casting starts, at 5-8cm 3 / s is poured into the water-cooled mold. The rapid pouring gives the melt a large momentum. When the high-temperature melt contacts the inner wall of the water-cooled mold, it first grows rapidly along the internal crystals. Therefore, the melt with a large momentum can impact the crystallization zone, forming broken grains that flow back into the melt, subsequently increasing the nucleation center to ensure that the ingot has a certain number of fine grains. Then, at 3-5cm 3 / s is poured into a water-cooled mold to reduce the casting speed, which can ensure that the subsequent growth of columnar crystals will not be broken. 3 / s is poured into a water-cooled mold and shrinkage compensation is completed slowly, which can reduce the depth of the riser.
[0010] (4) Cutting: Cutting the iridium ingot to obtain an iridium target blank;
[0011] (5) Rolling: Place the cut iridium target blank into an atmosphere heat treatment furnace, introduce a reducing atmosphere, heat to 1100-1450°C, and keep warm for 0.5-2h; then perform 3-6 passes of rolling, continuously introduce protective gas to cover the surface of the iridium target blank during the rolling process, and obtain a highly dense and highly oriented iridium target semi-finished product after the rolling process; heat treat the directionally solidified and cut iridium target blank, strictly control the surface temperature to be less than 1450°C, which can effectively control the surface activity of the ingot and ensure that it is not easy to oxidize. During the rolling process, continuously introduce protective gas to cover the surface of the ingot to reduce the contact between the surface of the ingot and oxygen and nitrogen, thereby controlling the thickness of the reaction layer of the final product, reducing the amount of machining and turning, and thereby controlling the loss rate to be less than 1‰. Compared with the traditional method of using a vacuum medium frequency induction heating furnace to produce iridium sputtering targets, the cost of producing iridium sputtering targets in this patent can be reduced by 10-20%, greatly reducing the price of iridium sputtering targets.
[0012] (6) Reduction: Place the semi-finished iridium target material into an atmosphere heat treatment furnace, introduce a reducing atmosphere, heat to 300-600°C, keep warm for 0.5-1h, and take it out after cooling in the furnace;
[0013] (7) Machining: machining the reduced iridium target semi-finished product to obtain the iridium sputtering target, wherein the mass loss rate of the iridium sputtering target is less than 1‰ compared with the iridium sheet in step (1).
[0014] Preferably, the protective gas in step (1) is one or more of helium, argon and xenon with a purity higher than 4N.
[0015] Preferably, the electromagnetic stirring time in step (2) is 5-15 min.
[0016] Preferably, the material of the water-cooling mold in step (3) is one of zirconium dioxide with a purity higher than 4N, high-purity iridium, copper, and aluminum oxide.
[0017] Preferably, the reducing atmosphere in step (6) is a hydrogen atmosphere, a carbon monoxide atmosphere, or a mixture of the two.
[0018] Preferably, in step (5), the rolling is carried out by strictly controlling the reduction of each rolling pass to 3-8%, and the iridium target blank is rotated 80°-100° after each rolling before the next rolling.
[0019] An iridium sputtering target prepared by the method of the present invention has a target surface showing a (111) crystal plane preferred orientation, a density of not less than 99.8%, a grain size of less than 300 μm, no internal defects, and a purity of not less than 4N.
[0020] Beneficial effects of the present invention:
[0021] (1) Compared with the vacuum medium frequency induction heating furnace, the present invention adopts the vacuum high frequency induction heating furnace to melt the iridium sheet. The vacuum high frequency induction heating furnace has the advantages of low cost, small footprint, fast heating rate, and small amount of material for single melting. Before the melting starts, the gas in the cavity is extracted and filled with protective gas to maintain 7×10 4 Pa-9×10 4 Pa, to prevent the melt from direct contact with air and oxidation, and at the same time fill in protective gas to reduce melt burning.
[0022] (2) The present invention performs heat treatment on the ingot obtained by directional solidification, strictly controls the surface temperature of the ingot to be less than 1450°C, controls the surface activity of the ingot to ensure that oxidation is not easy to occur, and continuously introduces protective gas to cover the surface of the ingot during the rolling process to reduce the contact between the surface of the ingot and oxygen and nitrogen, thereby controlling the thickness of the reaction layer of the final product, reducing the amount of machining and turning, and thereby controlling the loss rate to be less than 1‰. Compared with the traditional method of using a vacuum medium frequency induction heating furnace to produce iridium sputtering targets, the cost of producing iridium sputtering targets in this patent can be reduced by 10-20%, greatly reducing the price of iridium sputtering targets.
[0023] (3) The iridium sputtering target prepared by the method of the present invention has a face-centered cubic structure. The (111) crystal plane is a close-packed plane with weak bonding force among metal close-packed planes, which can effectively improve the sputtering rate at rated power. The iridium sputtering target surface presents a (111) crystal plane preferential orientation through directional solidification and rolling technology. This patent ultimately reduces the production cost of the iridium sputtering target while ensuring the performance of the iridium sputtering target. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 A physical picture of the iridium sputtering target prepared for the present invention;
[0025] Figure 2 Metallographic image of the iridium sputtering target prepared in the present invention. DETAILED DESCRIPTION
[0026] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. The embodiments shown below do not limit the invention content described in the claims. In addition, the entire contents of the structures represented by the following embodiments are not limited to those necessary as solutions to the invention described in the claims.
[0027] A method for preparing an iridium sputtering target with a low loss rate, wherein the target surface of the iridium sputtering target presents a (111) crystal plane preferred orientation, a density of not less than 99.8%, a grain size of less than 300 μm, no internal defects, and a purity of not less than 4N, comprising the following steps:
[0028] (1) Melting: Add iridium sheets with a purity of not less than 4N into a vacuum high-frequency induction heating furnace. Spread the iridium sheets tightly along the melting crucible and evacuate the furnace to 9×10 -4 -9×10 -3 Pa (e.g. 9.5×10 -4 Pa, 1×10 -3 Pa, 3×10 -3 Pa, 5×10 - 3 Pa, 7×10 -3 Pa, etc.), and then fill with protective gas until the vacuum degree is 7×10 4 Pa-9×10 4 Pa (e.g. 7.2×10 4 Pa, 7.5×10 4 Pa, 8×10 4 Pa, 8.5×10 4 Pa, etc.), smelting at a temperature of 2500-2700°C (e.g., 2520°C, 2550°C, 2580°C, 2600°C, 2620°C, 2650°C, 2680°C, etc.) to obtain an iridium melt; the protective gas is one or more of helium, argon, and xenon with a purity higher than 4N;
[0029] (2) Refining: The iridium melt is continuously heated in a vacuum high-frequency induction heating furnace, and the melt temperature is maintained at 2600-2700°C (e.g., 2620°C, 2640°C, 2660°C, 2680°C, etc.), and electromagnetic stirring is turned on for 5-15 minutes (e.g., 6 minutes, 8 minutes, 10 minutes, 12 minutes, 14 minutes, etc.);
[0030] (3) Directional solidification: Use a water-cooled mold with cooling water at the bottom to cast the iridium melt. The casting process is as follows: first, 5-8 cm 3 / s (e.g. 5.2cm 3 / s, 5.5cm 3 / s, 6.0cm 3 / s, 6.5cm 3 / s, 7.0cm 3 / s、7.5cm 3 / s, etc.) to 1 / 5-1 / 3 of the water-cooled mold; then slow down the casting speed to 3-5cm 3 / s (e.g. 3.2cm 3 / s, 3.5cm 3 / s, 3.8cm 3 / s, 4.0cm 3 / s, 4.2cm 3 / s, 4.5cm 3 / s, 4.8cm3 / s, etc.), cast to 2 / 5-3 / 5 of the water-cooled mold; then 1-2cm 3 / s (e.g. 1.2cm 3 / s, 1.4cm 3 / s, 1.5cm 3 / s, 1.6cm 3 / s, 1.8cm 3 / s, 1.9cm 3 / s, etc.) to slowly cast, and after the casting is completed and cooled, an ingot is obtained; when the casting is first started, the casting speed is 5-8cm 3 / s is poured into the water-cooled mold. The rapid pouring gives the melt a large momentum. When the high-temperature melt contacts the inner wall of the water-cooled mold, it first grows rapidly along the internal crystals. Therefore, the melt with a large momentum can impact the crystallization zone, forming broken grains that flow back into the melt, subsequently increasing the nucleation center to ensure that the ingot has a certain number of fine grains. Then, at 3-5cm 3 / s is poured into a water-cooled mold to reduce the casting speed, which can ensure that the subsequent growth of columnar crystals will not be broken. 3 / s is poured into the water-cooled mold, and the shrinkage is slowly completed, which can reduce the riser depth. The material of the water-cooled mold is one of zirconium dioxide with a purity higher than 4N, high-purity iridium, copper, and aluminum oxide;
[0031] (4) Cutting: Cutting the iridium ingot to obtain an iridium target blank;
[0032] (5) Rolling: placing the cut iridium target blank into an atmosphere heat treatment furnace, introducing a reducing atmosphere, heating to 1100-1450°C (e.g., 1150°C, 1200°C, 1250°C, 1300°C, 1350°C, 1400°C, etc.), and keeping warm for 0.5-2h (e.g., 0.6h, 0.8h, 1.0h, 1.2h, 1.5h, 1.8h, etc.); then performing 3-6 passes of rolling, strictly controlling the pass reduction of each rolling to 3-8%, rotating the iridium target blank by 80°-100° after each rolling before performing the next rolling, continuously introducing a protective gas to cover the surface of the iridium target blank during the rolling process, and obtaining a highly dense and highly oriented iridium target semi-finished product after the rolling is completed;
[0033] (6) Reduction: placing the semi-finished iridium target material into an atmosphere heat treatment furnace, introducing a reducing atmosphere, heating to 300-600°C (e.g., 350°C, 400°C, 450°C, 500°C, 550°C, etc.), keeping the temperature for 0.5-1h (e.g., 0.6h, 0.7h, 0.8h, 0.9h, etc.), cooling with the furnace and then taking it out; the reducing atmosphere is one of hydrogen and carbon monoxide atmospheres or a mixture of the two;
[0034] (7) Machining: machining the reduced iridium target semi-finished product to obtain the iridium sputtering target, wherein the mass loss rate of the iridium sputtering target is less than 1‰ compared with the iridium sheet in step (1).
[0035] Example 1
[0036] A method for preparing an iridium sputtering target with a low loss rate, wherein the specific preparation steps are as follows:
[0037] (1) Melting: 500g of iridium sheets with a purity of not less than 4N are placed in a vacuum high-frequency induction heating furnace. The iridium sheets are laid flat and tightly along the melting crucible. The vacuum degree in the furnace is reduced to 9×10 -4 Pa, close the vacuum valve, fill with protective gas to maintain the vacuum degree in the furnace at 8×10 4 Pa, start the vacuum high-frequency induction heating furnace, turn on the heating system, and quickly raise the temperature to 2600°C;
[0038] (2) Refining: The induction coil of the vacuum high-frequency induction heating furnace continuously heats the melt, maintaining the melt temperature at 2650°C, and starts electromagnetic stirring for 8 minutes;
[0039] (3) Directional solidification: Use a water-cooled mold with cooling water at the bottom to cast the iridium melt. The casting process is as follows: first, 5 cm 3 / s to 1 / 4 of the water-cooled mold; then slow down the casting speed to 3cm 3 / s, casting to 1 / 2 of the water-cooled mold; then 1cm 3 / s to slowly cast, and after the casting is completed and cooled, an ingot is obtained;
[0040] (4) Cutting: Cutting the ingot to obtain a target blank;
[0041] (5) Rolling: The cut target blank is placed in an atmosphere heat treatment furnace, introduced into a reducing atmosphere, heated to 1250°C, kept warm for 1 hour, and rolled four times, with the reduction of each pass strictly controlled at 4%. The target blank is rotated 90° after each rolling, and a protective gas is continuously introduced during the rolling process to cover the surface of the target blank, thereby obtaining a highly dense and highly oriented iridium semi-finished product;
[0042] (6) Reduction: Place the semi-finished product in an atmosphere heat treatment furnace, introduce a reducing atmosphere, heat to 400° C., keep warm for 0.6 hours, and take out the iridium semi-finished product after cooling in the furnace;
[0043] (7) Machining: The iridium semi-finished product is machined to obtain an iridium target as required, and the iridium debris generated by the machining is recovered.
[0044] The actual image of the iridium sputtering target finally obtained in this embodiment is shown in the attached figure. Figure 1The density of the iridium sputtering target was tested by the drainage method, and the relative density of the target was 99.98%. The grains of the iridium sputtering target were sampled and analyzed, and the metallographic diagram is shown in the attached figure. Figure 2 As shown, it can be observed that the grain size of the iridium sputtering target is uniform and within 300 μm. The final iridium sputtering target weighs 499.73 g and has a loss rate of 0.054%. The purity meets the 4N requirement after GDMS testing.
[0045] Example 2
[0046] A method for preparing an iridium sputtering target with a low loss rate, wherein the specific preparation steps are as follows:
[0047] (1) Melting: 240 g of iridium sheets with a purity of not less than 4N are placed in a vacuum high-frequency induction heating furnace. The iridium sheets are laid flat and tightly along the melting crucible. The vacuum degree in the furnace is reduced to 9×10 -4 Pa, close the vacuum valve, fill with protective gas to maintain the vacuum degree in the furnace at 9×10 4 Pa, start the vacuum high-frequency induction heating furnace, turn on the heating system, and quickly raise the temperature to 2500°C;
[0048] (2) Refining: The induction coil of the vacuum high-frequency induction heating furnace continuously heats the melt, maintaining the melt temperature at 2650°C, and starts electromagnetic stirring for 8 minutes;
[0049] (3) Directional solidification: Use a water-cooled mold with cooling water at the bottom to cast the iridium melt. The casting process is as follows: first, 8 cm 3 / s to 1 / 4 of the water-cooled mold; then slow down the casting speed to 5cm 3 / s, casting to 1 / 2 of the water-cooled mold; then 2cm 3 / s to slowly cast, and after the casting is completed and cooled, an ingot is obtained;
[0050] (4) Cutting: Cutting the ingot to obtain a target blank;
[0051] (5) Rolling: The cut target blank is placed in an atmosphere heat treatment furnace, introduced into a reducing atmosphere, heated to 1250°C, kept warm for 0.5 hours, and rolled three times, with the reduction of each pass strictly controlled at 3%. The target blank is rotated 90° after each rolling, and a protective gas is continuously introduced during the rolling process to cover the surface of the target blank, thereby obtaining a highly dense and highly oriented iridium semi-finished product;
[0052] (6) Reduction: Place the semi-finished product in an atmosphere heat treatment furnace, introduce a reducing atmosphere, heat to 400° C., keep warm for 0.6 hours, and take out the iridium semi-finished product after cooling in the furnace;
[0053] (7) Machining: The iridium semi-finished product is machined to obtain an iridium target as required, and the iridium debris generated by the machining is recovered.
[0054] The iridium sputtering target finally obtained in this embodiment is tested by the drainage method, and the relative density of the target is 99.98%. The grains of the iridium sputtering target are sampled and analyzed, and it can be observed that the grain size of the iridium sputtering target is uniform, and the grain size is within 300μm. The final iridium sputtering target weighs 239.82g, the loss rate is 0.075%, and the purity meets the 4N requirement after GDMS test.
[0055] Example 3
[0056] A method for preparing an iridium sputtering target with a low loss rate comprises the following steps:
[0057] (1) Melting: Add iridium sheets with a purity of not less than 4N into a vacuum high-frequency induction heating furnace. Spread the iridium sheets tightly along the melting crucible and evacuate the furnace to 7×10 -4 Pa, and then fill with protective gas to a vacuum degree of 8×10 4 Pa, smelting at a temperature of 2500°C to obtain an iridium melt; the protective gas is helium with a purity higher than 4N;
[0058] (2) Refining: The iridium melt is continuously heated in a vacuum high-frequency induction heating furnace, the melt temperature is maintained at 2600°C, and electromagnetic stirring is turned on for 5 minutes;
[0059] (3) Directional solidification: Use a water-cooled mold with cooling water at the bottom to cast the iridium melt. The casting process is as follows: first, 3 / s to 1 / 5 of the water-cooled mold; then slow down the casting speed to 3.5cm 3 / s, casting to 2 / 5 of the water-cooled mold; then 1.2cm 3 / s is slowly cast, and after the casting is completed and cooled, an ingot is obtained; the material of the water-cooling mold is zirconium dioxide with a purity higher than 4N;
[0060] (4) Cutting: Cutting the iridium ingot to obtain an iridium target blank;
[0061] (5) Rolling: The cut iridium target blank is placed in an atmosphere heat treatment furnace, introduced into a reducing atmosphere, heated to 1100°C, and kept warm for 0.5 h; then three passes of rolling are performed, and the reduction amount of each rolling pass is strictly controlled to be 3%. After each rolling, the iridium target blank is rotated 88° before the next rolling. During the rolling process, a protective gas is continuously introduced to cover the surface of the iridium target blank. After the rolling is completed, a highly dense and highly oriented iridium target semi-finished product is obtained;
[0062] (6) Reduction: placing the semi-finished iridium target material into an atmosphere heat treatment furnace, introducing a reducing atmosphere, heating to 300° C., keeping the temperature for 0.5 h, and taking it out after cooling with the furnace; the reducing atmosphere is one of hydrogen and carbon monoxide atmospheres or a mixture of the two;
[0063] (7) Machining: machining the reduced iridium target semi-finished product to obtain the iridium sputtering target.
[0064] The iridium sputtering target finally prepared in this embodiment is tested by the drainage method, and the relative density of the target is ≥99.82%. The grains of the iridium sputtering target are sampled and analyzed, and it can be observed that the grain size of the iridium sputtering target is uniform, the grain size is within 300 μm, and the loss rate is 0.55‰. The purity meets the 4N requirement after GDMS test.
[0065] Example 4
[0066] A method for preparing an iridium sputtering target with a low loss rate comprises the following steps:
[0067] (1) Melting: Add iridium sheets with a purity of not less than 4N into a vacuum high-frequency induction heating furnace. Spread the iridium sheets tightly along the melting crucible and evacuate the furnace to 9×10 -3 Pa, and then fill with protective gas to a vacuum degree of 9×10 4 Pa, smelted at a temperature of 2700°C to obtain an iridium melt; the protective gas is argon with a purity higher than 4N;
[0068] (2) Refining: The iridium melt is continuously heated in a vacuum high-frequency induction heating furnace, the melt temperature is maintained at 2700°C, and electromagnetic stirring is turned on for 15 minutes;
[0069] (3) Directional solidification: Use a water-cooled mold with cooling water at the bottom to cast the iridium melt. The casting process is as follows: first, 7 cm 3 / s to 1 / 3 of the water-cooled mold; then slow down the casting speed to 4cm 3 / s, casting to 3 / 5 of the water-cooled mold; then 1.5cm 3 / s, and slowly casting is performed to obtain an ingot after the casting is completed and cooled; the material of the water-cooling mold is high-purity iridium with a purity higher than 4N;
[0070] (4) Cutting: Cutting the iridium ingot to obtain an iridium target blank;
[0071] (5) Rolling: The cut iridium target blank is placed in an atmosphere heat treatment furnace, introduced into a reducing atmosphere, heated to 1450°C, and kept warm for 2 hours; then 6 passes of rolling are performed, and the reduction amount of each rolling pass is strictly controlled to be 8%. After each rolling, the iridium target blank is rotated 98° before the next rolling. During the rolling process, a protective gas is continuously introduced to cover the surface of the iridium target blank. After the rolling is completed, a highly dense and highly oriented iridium target semi-finished product is obtained;
[0072] (6) Reduction: placing the semi-finished iridium target material into an atmosphere heat treatment furnace, introducing a reducing atmosphere, heating to 600° C., keeping the temperature for 1 hour, and taking it out after cooling with the furnace; the reducing atmosphere is carbon monoxide;
[0073] (7) Machining: machining the reduced iridium target semi-finished product to obtain the iridium sputtering target.
[0074] The iridium sputtering target finally prepared in this embodiment is tested by the drainage method, and the relative density of the target is ≥99.95%. The grains of the iridium sputtering target are sampled and analyzed, and it can be observed that the grain size of the iridium sputtering target is uniform, the grain size is within 300 μm, the loss rate is 0.87‰, and the purity meets the 4N requirement after GDMS test.
[0075] Example 5
[0076] A method for preparing an iridium sputtering target with a low loss rate comprises the following steps:
[0077] (1) Melting: Add iridium sheets with a purity of not less than 4N into a vacuum high-frequency induction heating furnace. Spread the iridium sheets tightly along the melting crucible and evacuate the furnace to 2×10 -3 Pa, and then fill with protective gas to a vacuum degree of 7.5×10 4 Pa, smelted at a temperature of 2550°C to obtain an iridium melt; the protective gas is xenon with a purity higher than 4N;
[0078] (2) Refining: The iridium melt is continuously heated in a vacuum high-frequency induction heating furnace, the melt temperature is maintained at 2620°C, and electromagnetic stirring is turned on for 6 minutes;
[0079] (3) Directional solidification: Use a water-cooled mold with cooling water at the bottom to cast the iridium melt. The casting process is as follows: first, 7.5 cm 3 / s to 1 / 4 of the water-cooled mold; then slow down the casting speed to 4.5cm 3 / s, casting to 1 / 2 of the water-cooled mold; then 1.5cm 3 / s is slowly cast, and after the casting is completed and cooled, an ingot is obtained; the material of the water-cooling mold is copper with a purity higher than 4N;
[0080] (4) Cutting: Cutting the iridium ingot to obtain an iridium target blank;
[0081] (5) Rolling: The cut iridium target blank is placed in an atmosphere heat treatment furnace, introduced into a reducing atmosphere, heated to 1150°C, and kept warm for 1 hour; then four rolling passes are performed, and the reduction amount of each rolling pass is strictly controlled to be 4%. After each rolling, the iridium target blank is rotated 90° before the next rolling. During the rolling process, a protective gas is continuously introduced to cover the surface of the iridium target blank. After the rolling is completed, a highly dense and highly oriented iridium target semi-finished product is obtained;
[0082] (6) Reduction: placing the semi-finished iridium target material into an atmosphere heat treatment furnace, introducing a reducing atmosphere, heating to 400° C., keeping the temperature for 0.6 h, and taking it out after cooling with the furnace; the reducing atmosphere is a mixture of hydrogen and carbon monoxide atmosphere;
[0083] (7) Machining: machining the reduced iridium target semi-finished product to obtain the iridium sputtering target.
[0084] The iridium sputtering target finally prepared in this embodiment is tested by the drainage method, and the relative density of the target is ≥99.93%. The grains of the iridium sputtering target are sampled and analyzed, and it can be observed that the grain size of the iridium sputtering target is uniform, the grain size is within 300 μm, the loss rate is 0.51‰, and the purity meets the 4N requirement after GDMS test.
[0085] Example 6
[0086] A method for preparing an iridium sputtering target with a low loss rate comprises the following steps:
[0087] (1) Melting: Add iridium sheets with a purity of not less than 4N into a vacuum high-frequency induction heating furnace. Spread the iridium sheets tightly along the melting crucible and evacuate the furnace to 5×10 -3 Pa, and then fill with protective gas to a vacuum degree of 8.5×10 4 Pa, smelting at 2600°C to obtain iridium melt; the protective gas is a mixture of helium, argon and xenon with a purity higher than 4N
[0088] (2) Refining: The iridium melt is continuously heated in a vacuum high-frequency induction heating furnace, the melt temperature is maintained at 2680°C, and electromagnetic stirring is turned on for 12 minutes;
[0089] (3) Directional solidification: Use a water-cooled mold with cooling water at the bottom to cast the iridium melt. The casting process is as follows: first, 8 cm 3 / s to 1 / 4 of the water-cooled mold; then slow down the casting speed to 3.3cm 3 / s, casting to 1 / 2 of the water-cooled mold; then 1.8cm 3 / s is slowly cast, and after the casting is completed and cooled, an ingot is obtained; the material of the water-cooling mold is alumina with a purity higher than 4N;
[0090] (4) Cutting: Cutting the iridium ingot to obtain an iridium target blank;
[0091] (5) Rolling: The cut iridium target blank is placed in an atmosphere heat treatment furnace, introduced into a reducing atmosphere, heated to 1400°C, and kept warm for 1.5 hours; then 5 passes of rolling are performed, and the reduction amount of each rolling pass is strictly controlled to be 3-8%. After each rolling, the iridium target blank is rotated 90° before the next rolling. During the rolling process, a protective gas is continuously introduced to cover the surface of the iridium target blank. After the rolling is completed, a highly dense and highly oriented iridium target semi-finished product is obtained;
[0092] (6) Reduction: placing the semi-finished iridium target material into an atmosphere heat treatment furnace, introducing a reducing atmosphere, heating to 500° C., keeping the temperature for 0.8 h, and taking it out after cooling in the furnace; the reducing atmosphere is one of hydrogen and carbon monoxide atmospheres or a mixture of the two;
[0093] (7) Machining: machining the reduced iridium target semi-finished product to obtain the iridium sputtering target.
[0094] The iridium sputtering target finally prepared in this embodiment is tested by the drainage method, and the relative density of the target is ≥99.95%. The grains of the iridium sputtering target are sampled and analyzed, and it can be observed that the grain size of the iridium sputtering target is uniform, the grain size is within 300 μm, the loss rate is 0.61‰, and the purity meets the 4N requirement after GDMS test.
[0095] Comparative Example 1
[0096] A method for preparing an iridium sputtering target, the specific preparation steps are as follows:
[0097] (1) Melting: 240 g of iridium sheets with a purity of not less than 4N are placed in a vacuum high-frequency induction heating furnace. The iridium sheets are laid flat and tightly along the melting crucible. The vacuum degree in the furnace is maintained at 9×10 -3 Pa-9×10 -4 Pa, start the vacuum high-frequency induction heating furnace, turn on the heating system, and quickly raise the temperature to 2500°C;
[0098] (2) Refining: The induction coil of the vacuum high-frequency induction heating furnace continuously heats the melt, maintaining the melt temperature at 2650°C, and starts electromagnetic stirring for 8 minutes;
[0099] (3) Directional solidification: When casting the melt, a water-cooled mold with cooling water at the bottom is used. During casting, the casting speed is controlled to first quickly pour to 1 / 4 of the water-cooled mold, then slow down the casting speed to pour to 1 / 2 of the water-cooled mold and then slowly cast to obtain an ingot after cooling;
[0100] (4) Cutting: Cutting the ingot to obtain a target blank;
[0101] (5) Rolling: The cut target blank is placed in an atmosphere heat treatment furnace, introduced into a reducing atmosphere, heated to 1250°C, kept warm for 0.5 hours, and rolled three times, with the reduction of each pass strictly controlled at 3%. The target blank is rotated 90° after each rolling, and a protective gas is continuously introduced during the rolling process to cover the surface of the target blank, thereby obtaining a highly dense and highly oriented iridium semi-finished product;
[0102] (6) Reduction: Place the semi-finished product in an atmosphere heat treatment furnace, introduce a reducing atmosphere, heat to 400° C., keep warm for 0.6 hours, and take out the iridium semi-finished product after cooling in the furnace;
[0103] (7) Machining: The iridium semi-finished product is machined to obtain an iridium target as required, and the iridium debris generated by the machining is recovered.
[0104] The iridium sputtering target finally obtained in this comparative example 1 was tested by the drainage method, and the relative density of the target was 99.96%. The grains of the iridium sputtering target were sampled and analyzed, and it was observed that the grain size of the iridium sputtering target was uniform, and the grain size was within 300μm. The final iridium sputtering target weighed 237.15g and the loss rate was 1.1875%. After GDMS testing, the purity met the 4N requirement.
[0105] Failure to add protective gas to increase the pressure during the smelting process will increase the volatilization rate of iridium, causing higher losses and significantly increasing production costs. Therefore, appropriate protective gas should be added during the smelting process.
[0106] Comparative Example 2
[0107] A method for preparing an iridium sputtering target, the specific preparation steps are as follows:
[0108] (1) Melting: 240 g of iridium sheets with a purity of not less than 4N are placed in a vacuum high-frequency induction heating furnace. The iridium sheets are laid flat and tightly along the melting crucible. The vacuum degree in the furnace is reduced to 9×10 -4 Pa, close the vacuum valve, fill with protective gas to maintain the vacuum degree in the furnace at 9×10 4 Pa, start the vacuum high-frequency induction heating furnace, turn on the heating system, and quickly raise the temperature to 2500°C;
[0109] (2) Refining: The induction coil of the vacuum high-frequency induction heating furnace continuously heats the melt, maintaining the melt temperature at 2650°C, and starts electromagnetic stirring for 8 minutes;
[0110] (3) Directional solidification: When casting the melt, a water-cooled mold with cooling water at the bottom is used. During casting, the casting speed is controlled to first quickly pour to 1 / 4 of the water-cooled mold, then slow down the casting speed to pour to 1 / 2 of the water-cooled mold and then slowly cast to obtain an ingot after cooling;
[0111] (4) Cutting: Cutting the ingot to obtain a target blank;
[0112] (5) Rolling: The cut target blank is placed in a heat treatment furnace, heated to 1250°C, kept warm for 0.5 hours, and rolled three times, with the reduction of each pass strictly controlled at 3%. The target blank is rotated 90° each time rolling to obtain a highly dense and highly oriented iridium semi-finished product;
[0113] (6) Reduction: Place the semi-finished product in an atmosphere heat treatment furnace, introduce a reducing atmosphere, heat to 400° C., keep warm for 0.6 hours, and take out the iridium semi-finished product after cooling in the furnace;
[0114] (7) Machining: The iridium semi-finished product is machined to obtain an iridium target as required, and the iridium debris generated by the machining is recovered.
[0115] The iridium sputtering target finally prepared in this comparative example 2 was tested by the drainage method, and the relative density of the target was 99.97%. The grains of the iridium sputtering target were sampled and analyzed, and it can be observed that the grain size of the iridium sputtering target is uniform, and the grain size is within 300 μm. The final iridium sputtering target weighs 238.22g, and the loss rate is 0.742%. The purity meets the 4N requirement after GDMS testing.
[0116] During the rolling process, no atmosphere heat treatment furnace is used for heating, and no protective gas is used to cover the surface of the target blank. During the heating process, the surface of the target blank will react. After rolling, the surface oxide layer will detach due to the effects of the stress field and temperature field, and the loss rate will increase.
[0117] Comparative Example 3
[0118] The difference between this comparative example and Example 1 is that the uniform casting rate in step (3) is 4.5 cm 3 / s, other conditions being the same.
[0119] The iridium sputtering target material finally prepared in this comparative example was tested by the water displacement method, and the relative density of the target material was 99.36%, and the loss rate of the iridium sputtering target material was 4.1%.
[0120] Comparative Example 4
[0121] The difference between this comparative example and Example 2 is that the uniform casting speed of 10 cm in step (3) is 3 / s, other conditions being the same.
[0122] The iridium sputtering target material finally prepared in this comparative example was tested by the water displacement method, and the relative density of the target material was 99.01%, and the loss rate of the iridium sputtering target material was 4.6%.
[0123] Comparative Example 5
[0124] The difference between this comparative example and Example 3 is that the directional solidification casting process is: first, 3 / s; then slow down the casting speed to 8cm 3 / s; then 1cm 3 The casting is slowly performed at a rate of 1:1 / s. After the casting is completed and cooled, an ingot is obtained. Other conditions are the same.
[0125] The iridium sputtering target material finally prepared in this comparative example was tested by the drainage method, and the relative density of the target material was 99.43%. The grains of the iridium sputtering target material were sampled and analyzed, and it was observed that the grain size of the iridium sputtering target material was uniform, and the grain size was within 300 μm, and the loss rate of the iridium sputtering target material was finally obtained to be 2.3%.
[0126] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing an iridium sputtering target with a low loss rate, characterized in that: The following steps are involved: (1) Melting: Place iridium sheets with a purity of not less than 4N into a vacuum high-frequency induction heating furnace and first evacuate to 9×10 -4 Pa-9×10 -3 Pa, and then fill with protective gas to a vacuum degree of 7×10 4 Pa-9×10 4 Pa, smelted at 2500-2700°C to obtain iridium melt; (2) Refining: The iridium melt is continuously heated in a vacuum high-frequency induction heating furnace, the melt temperature is maintained at 2600-2700°C, and electromagnetic stirring is turned on; (3) Directional solidification: Use a water-cooled mold with cooling water at the bottom to cast the iridium melt. The casting process is as follows: first, 5-8 cm 3 / s to 1 / 5-1 / 3 of the water-cooled mold; then slow down the casting speed to 3-5cm 3 / s, casting to 2 / 5-3 / 5 of the water-cooled mold; then 1-2cm 3 / s to slowly cast, and after the casting is completed and cooled, an ingot is obtained; (4) Cutting: Cutting the iridium ingot to obtain an iridium target blank; (5) Rolling: The cut iridium target blank is placed in an atmosphere heat treatment furnace, introduced into a reducing atmosphere, heated to 1100-1450°C, and kept warm for 0.5-2h; then rolled for 3-6 times, during which a protective gas is continuously introduced to cover the surface of the iridium target blank, and after the rolling is completed, a highly dense and highly oriented iridium target semi-finished product is obtained; (6) Reduction: Place the semi-finished iridium target material into an atmosphere heat treatment furnace, introduce a reducing atmosphere, heat to 300-600°C, keep warm for 0.5-1h, and take it out after cooling in the furnace; (7) Machining: machining the reduced iridium target semi-finished product to obtain the iridium sputtering target, wherein the mass loss rate of the iridium sputtering target is less than 1‰ compared with the iridium sheet in step (1).
2. The method for preparing an iridium sputtering target with a low loss rate according to claim 1, characterized in that: The protective gas in steps (1) and (5) is one or more of helium, argon and xenon with a purity higher than 4N.
3. The method for preparing an iridium sputtering target with a low loss rate according to claim 1, characterized in that: The electromagnetic stirring time in step (2) is 5-15 min.
4. The method for preparing an iridium sputtering target with a low loss rate according to claim 1, characterized in that: The material of the water-cooling mold in step (3) is one of zirconium dioxide with a purity higher than 4N, high-purity iridium, copper, and aluminum oxide.
5. The method for preparing an iridium sputtering target with a low loss rate according to claim 1, characterized in that: The reducing atmosphere in steps (5) and (6) is a hydrogen atmosphere, a carbon monoxide atmosphere, or a mixture of the two.
6. The method for preparing an iridium sputtering target with low loss rate according to any one of claims 1 to 5, characterized in that: In step (5), the rolling is performed by strictly controlling the reduction of each rolling pass to 3-8%, and the iridium target blank is rotated 80°-100° after each rolling before the next rolling.
7. An iridium sputtering target prepared by the method according to any one of claims 1 to 6, characterized in that: The target surface of the iridium sputtering target presents a (111) crystal plane preferred orientation, a density of not less than 99.8%, a grain size of less than 300 μm, no internal defects, and a purity of not less than 4N.
Citation Information
Patent Citations
Iridium sputtering target material with crystal grain high-orienteering orientation and preparation method thereof
CN111235536A
Production of high purity iridium or ruthenium sputtering target
JP1997041131A
Manufacturing method of the iridium and ruthenium sputtering target having a fine grain size
KR1020080049454A
Magnetic sputter targets manufactured using directional solidification
US20070169853A1
Cited By
CoFeV alloy target material and preparation method thereof
CN119609577A
Preparation method of high-purity iridium target material
CN121776505A