Preparation device and preparation method of organic semiconductor film
By using tubular channels and inert gas-carrying raw material deposition methods in the preparation of organic semiconductor thin films, the problems of large amount of raw materials and complex operation are solved, and efficient and economical film preparation is achieved, suitable for a variety of substrates and improved film performance.
Patent Information
- Application Number
- CN202411014422.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
AI Technical Summary
In the existing organic semiconductor thin film preparation methods, the amount of coating raw materials is used relatively large, the raw material is inadequate, and the vacuum coating method requires expensive vacuum evacuation equipment and complex operations.
A preparation device including a tube channel, a raw material bearing device and a heating device is designed to evaporate and deposit the raw material by carrying the raw material through an inert gas. A program heating and gas reflux device is used to uniformly deposit the raw material, reducing the amount of raw material and simplifying the operation.
It realizes savings in raw material usage, reduces the difficulty of preparation, is suitable for a variety of coating substrates, avoids complex operations of vacuum coating methods, and improves the uniformity and performance of the film.
Smart Images

Figure CN118969667A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of organic thin film manufacturing, and in particular to a device and method for preparing an organic semiconductor thin film. Background Art
[0002] Organic semiconductor materials are widely used in the field of optoelectronic devices due to their advantages such as easy structural modification, large-area processing, high mechanical flexibility, tailorability, simple process and low production cost. With the vigorous development of the flexible electronics industry in recent years, organic semiconductor films have been increasingly valued by researchers from various countries. Due to their unique properties, organic semiconductor film materials have shown wide application potential in many fields. For example, organic thin film transistors are widely used in flexible circuits, displays and sensors. In addition, the flexibility and adjustability of organic semiconductor films make them suitable for the development of smart sensors, which can be used in many fields such as environmental monitoring and health monitoring. For example, the transparency and flexibility of organic semiconductor films make them suitable for the manufacture of RFID tags, which can be used for product tracking and management.
[0003] At present, the commonly used methods for preparing organic semiconductor thin films are: chemical vapor deposition, solution deposition film formation and vacuum coating. The solvent method requires less raw materials, but its limitation is that the organic semiconductor material needs to be soluble or have a soluble precursor, and the purity of the prepared film is low. The heating temperature required for the chemical vapor deposition method is relatively high, usually between 850 and 1100 ° C. This method is not suitable for materials that are not resistant to high temperatures. In addition, the complexity of the chemical vapor deposition operation and the high requirements for equipment and operation also limit its application. Vacuum coating is one of the commonly used methods for obtaining high-performance thin films at this stage. It is to prepare organic thin films by thermal evaporation, sputtering and organic molecular epitaxial growth under high vacuum or ultra-high vacuum conditions. It is a commonly used method for obtaining high-performance thin films at this stage. However, the method of preparing organic thin films in vacuum has relatively high requirements for equipment, requires expensive vacuum equipment, is complex to operate and requires a large amount of organic materials. Summary of the invention
[0004] In view of the above-mentioned shortcomings of the prior art, the purpose of the present invention is to provide an organic semiconductor film preparation device and a preparation method thereof, which are used to solve the problems existing in the prior art in the preparation process of organic semiconductor films, such as large amount of coating raw materials, insufficient solubility of raw materials, and expensive and complicated vacuum equipment.
[0005] The first aspect of the present invention provides a device for preparing an organic semiconductor film, comprising: a tubular channel, a raw material supporting device, a heating device and a gas pipeline; the gas pipeline is connected to the gas inlet end of the tubular channel; the raw material supporting device is located in the tubular channel for supporting the raw material, and the heating device is used to heat the raw material.
[0006] In some specific embodiments, the raw material supporting device is a quartz tube, and the aperture of the air inlet of the quartz tube is larger than the aperture of the air outlet.
[0007] In some specific embodiments, the diameter of the gas inlet of the quartz tube is 1.5 to 3 times the diameter of the gas outlet.
[0008] Preferably, the diameter of the air inlet of the quartz tube is twice the diameter of the air outlet.
[0009] In some specific implementations, a gas flow meter is provided on the gas pipeline.
[0010] In some specific implementations, a pressure gauge is provided on the gas pipeline.
[0011] In some specific embodiments, a gas valve is provided on the gas pipeline.
[0012] In some specific embodiments, furnace plugs for heat preservation are provided at both ends of the tubular channel.
[0013] Preferably, the furnace plug allows the airflow in the tubular channel to pass through without allowing solid matter in the pipe to pass through.
[0014] In some specific embodiments, the preparation device further comprises a base support, and the base support is disposed in the tubular channel, and along the gas flow direction, the base support is located downstream of the raw material supporting device.
[0015] Preferably, the base support is arranged at the far end of the heating zone.
[0016] A second aspect of the present invention provides a method for preparing an organic semiconductor thin film, comprising the following steps:
[0017] 1) placing a substrate into a tubular channel, arranged downstream of the raw material supporting device, and placing the substrate into the raw material supporting device;
[0018] 2) Inert gas is introduced from the gas pipeline to maintain an inert gas flow channel from the gas inlet end to the gas outlet end in the tubular channel, and a heating device is used to heat the raw material. After the raw material evaporates, it is carried by the inert gas and deposited on the substrate surface;
[0019] 3) After the deposition is completed, the heating is stopped to obtain an organic semiconductor film on the surface of the substrate.
[0020] In some specific embodiments, the raw material is a small molecule compound, an oligomer and a derivative thereof having a conjugated structure, preferably any one of thiophene, pyrrole, carbazole, aniline, fluorene and condensed aromatic hydrocarbons.
[0021] Preferably, the condensed aromatic hydrocarbon is any one selected from tetracene, pentacene, a tetracene derivative or a pentacene derivative.
[0022] In some specific embodiments, the substrate is any one of metal foil, glass, silicon wafer, plastic, diamond, and sapphire.
[0023] In some specific embodiments, the uniformity of the organic semiconductor thin film is regulated by adjusting the flow rate of the inert gas.
[0024] In some specific embodiments, the thickness of the organic semiconductor film is controlled by adjusting the deposition time.
[0025] In some specific embodiments, the heating temperature is lower than the melting point of the raw material.
[0026] In some specific embodiments, the heating temperature is 250-350°C.
[0027] In some specific embodiments, the heating temperature is 280-300°C; for example, it can be 280°C, 285°C, 290°C, 295°C or 300°C.
[0028] In some specific embodiments, the heating is programmed temperature heating.
[0029] Preferably, the initial temperature of the programmed temperature increase is 20-40°C.
[0030] Preferably, the heating rate of the programmed temperature is 5 to 20° C. / min.
[0031] In some specific embodiments, the nitrogen flow rate is 5 to 300 ml / min.
[0032] In some specific embodiments, the nitrogen flow rate is 5 to 50 ml / min; for example, it can be 5 ml / min, 10 ml / min, 15 ml / min, 20 ml / min, 25 ml / min, 30 ml / min, 35 ml / min, 40 ml / min or 50 ml / min.
[0033] In some specific embodiments, the nitrogen flow rate is 50-100 ml / min; for example, it can be 60 ml / min, 65 ml / min, 70 ml / min, 75 ml / min, 80 ml / min, 85 ml / min, 90 ml / min, 95 ml / min or 100 ml / min.
[0034] In some specific embodiments, the nitrogen flow rate is 100-200 ml / min; for example, it can be 110 ml / min, 120 ml / min, 130 ml / min, 140 ml / min, 150 ml / min, 160 ml / min, 170 ml / min, 180 ml / min, 190 ml / min or 200 ml / min.
[0035] In some specific embodiments, the nitrogen flow rate is 200-300 ml / min; for example, it can be 210 ml / min, 220 ml / min, 230 ml / min, 240 ml / min, 250 ml / min, 260 ml / min, 270 ml / min, 280 ml / min, 290 ml / min or 300 ml / min.
[0036] In some specific embodiments, the heating time is 4 to 10 hours.
[0037] In some specific embodiments, the heating time is 4 to 8 hours.
[0038] In some specific embodiments, the heating time is 5 to 8 hours.
[0039] In some specific embodiments, the heating time is 5 to 6 hours.
[0040] A third aspect of the present invention provides a method for screening raw materials for preparing organic semiconductor thin films.
[0041] As described above, the organic semiconductor thin film preparation device and preparation method of the present invention have the following beneficial effects:
[0042] 1. This application adopts programmed heating and continuously introduces inert gas during the heating process, so that the organic semiconductor material evaporates slowly due to heat and is carried by the inert gas to the surface of the substrate to deposit and form a thin film. The inert gas can also protect the organic matter from being oxidized.
[0043] 2. The present application designs a gas reflux device, in which the gas refluxes in the raw material carrying device, so that the raw material carried by the gas is deposited more evenly, thus saving the amount of raw material. The vacuum coating method requires the raw material to be pressed into sheets and then evaporated, which requires at least 5g of raw material. The present application adopts a reflux device, and a uniform thin film can be obtained with as little as 10mg of raw material.
[0044] 3. The device of the present application has a simple structure and is easy to operate. It is suitable for a variety of coating substrates and can avoid complicated operations such as vacuuming in vacuum coating methods, greatly reducing the technical difficulty of coating and being more economical and practical.
[0045] 4. The device of the present application is suitable for coating most small molecule compounds used to prepare organic semiconductor materials, especially for raw materials with poor solubility that cannot be formed into films using solution deposition methods. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 It is a schematic diagram of a device for preparing an organic semiconductor thin film according to the present invention.
[0047] Figure 2 Shown is a schematic diagram of a base support of the present invention.
[0048] Figure 3 It is a schematic diagram showing a substrate supporting a substrate in Embodiment 1 of the present invention.
[0049] Figure 4 (a) is a microscope picture of a pentacene film deposited on a diamond anvil in Example 1 of the present invention, and (b) is a microscope picture of a film on the left side of the diamond anvil after it has been erased.
[0050] Figure 5 It is a schematic diagram of the sample chamber when a high pressure experimental test is performed on a pentacene film deposited on a diamond anvil in Example 1 of the present invention.
[0051] Figure 6 Shown are the steady-state absorption spectrum results of the pentacene film on the diamond anvil cell in Example 1 of the present invention.
[0052] Figure 7 Shown is the XRD diffraction pattern of the pentacene film on the diamond anvil cell in Example 2 of the present invention.
[0053] Figure 8 Shown are the results of scanning electron microscopy observation of the pentacene film on the diamond anvil cell in Example 2 of the present invention.
[0054] Fig. 9 Shown are the XRD characterization results of rubrene powder and rubrene film on sapphire substrate in Example 3 of the present invention, wherein Powder represents rubrene powder and Film represents rubrene film.
[0055] Fig.10 Shown are the results of atomic force microscopy observation of the rubrene film on the sapphire substrate in Example 3 of the present invention.
[0056] Fig.11 A microscope picture showing the position of sapphire fragments coated with rubrene film placed in the sample cavity in Example 3 of the present invention.
[0057] Fig.12 It is a schematic diagram showing the position of placing sapphire fragments coated with rubrene film in the raw material chamber in Example 2 of the present invention.
[0058] Fig.13 Shown are the steady-state absorption spectra of the rubrene film on the sapphire substrate under different pressures in Example 2 of the present invention.
[0059] Description of Figure Numbers
[0060] 1-gas flow meter; 2-flange; 3-pressure gauge; 4-tubular channel; 5-furnace plug; 6-raw material; 7-raw material carrying device; 8-heating device; 9-base support; 10-gas valve. DETAILED DESCRIPTION
[0061] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0062] In addition, it should be understood that one or more method steps mentioned in the present invention do not exclude the existence of other method steps before or after the combination step or the insertion of other method steps between these explicitly mentioned steps, unless otherwise specified; it should also be understood that the combination connection relationship between one or more devices / apparatuses mentioned in the present invention does not exclude the existence of other devices / apparatuses before or after the combination device / apparatus or the insertion of other devices / apparatuses between these explicitly mentioned two devices / apparatuses, unless otherwise specified. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or the scope of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the present invention without substantially changing the technical content.
[0063] The organic semiconductor thin film preparation device used in the present application is convenient, simple, easy to operate, requires a small amount of raw materials, and the prepared thin film has high performance.
[0064] like Figure 1 As shown, the present invention provides a device for preparing an organic semiconductor film, including a tubular channel 4, a raw material supporting device 7, a heating device 8 and a gas pipeline; the gas pipeline is connected to the tubular channel 4 for introducing gas into the tubular channel 4, the raw material supporting device 7 is located in the tubular channel 4 for supporting the raw material 6, and the heating device 8 is used to heat the raw material 6.
[0065] In a further embodiment, the tubular channel 4 is a quartz tube.
[0066] In a specific embodiment, the raw material carrying device 7 is a quartz tube with inconsistent openings at both ends, and the aperture of the air inlet of the quartz tube is larger than the aperture of the air outlet; during the gas circulation process, the gas refluxes in the quartz tube, making the raw material 6 carried by the gas deposited more evenly, saving the amount of raw material 6.
[0067] In a more specific embodiment, the aperture of the gas inlet of the quartz tube is twice the aperture of the gas outlet.
[0068] In a specific embodiment, a gas flow meter 1 is provided on the gas pipeline; during the gas circulation process, the gas flow meter 1 is used to observe the flow rate of the gas.
[0069] In a specific embodiment, a barometer 3 is provided on the gas pipeline; during the gas circulation process, the barometer 3 is used to observe the gas pressure of the system to prevent the tubular channel from rupturing due to excessive system pressure.
[0070] In a specific embodiment, a gas valve 10 is provided on the gas pipeline, and the gas valve 10 is a one-way flow valve; during the gas circulation process, the gas introduced into the gas pipeline can flow in and out through the gas valve 10, but the external gas cannot flow into the system through the gas valve 10.
[0071] In a specific embodiment, furnace plugs 5 are provided at both ends of the tubular channel. The furnace plugs 5 are provided at both ends of the tubular channel 4. The furnace plugs 5 can allow the airflow in the tubular channel 4 to pass through the furnace plugs 5; the furnace plugs 5 can have a heat-insulating effect to maintain the temperature in the tubular channel 4; in addition, the furnace plugs 5 can also play a safety role to prevent the base support 9 and the raw materials from being blown out of the system under a larger airflow.
[0072] In a Figure 1 and Figure 2 In the specific embodiment shown, a substrate support 9 for supporting the substrate is provided in the tubular channel 4 at the gas outlet end of the raw material supporting device.
[0073] In a specific embodiment, the base support 9 is located at the far end of the heating zone.
[0074] In a specific embodiment, a substrate mounting through hole is provided at the top of the substrate holder 9, and the through hole matches the size of the substrate; when in use, the substrate is installed in the through hole, and then the substrate holder 9 carrying the substrate is placed in the tubular channel 4; there is a certain gap between the upper end of the substrate holder 9 and the inner wall of the tubular channel 4; during the thin film deposition process, the raw material molecules will exist in a large amount in the cavity of the tubular channel 4 after sublimation, and will be evenly deposited on the substrate located on the substrate holder 9 through gas transport.
[0075] In a specific embodiment, there is a gap of 5 to 10 mm between the upper end of the base support 9 and the inner wall of the tubular channel 4 .
[0076] In a specific embodiment, the base support 9 is annular, and its size matches the inner diameter of the tubular channel 4. The surface of the base support is frosted. Therefore, during the film preparation process, the friction between the bottom of the base support and the inner wall of the tubular channel 4 fixes it in the tubular channel 4 and does not move.
[0077] In a specific embodiment, the air tightness of the device needs to be checked before thin film preparation to ensure that the entire system is airtight and leak-proof, so as to facilitate accurate control of the gas flow rate during the subsequent thin film preparation process.
[0078] Example 1
[0079] This embodiment uses the above device to prepare a pentacene film on a diamond anvil cell substrate. Specifically, the following steps are included:
[0080] Step 1, use a type IIa diamond anvil with an 800 micron table (purchased from Shanghai Zhenyuan Materials Technology Co., Ltd.), the diamond diameter is 3.5mm, fixed on a 12mm silicon carbide pad as anvil. The glue used for fixing and the diamond will not be deformed or oxidized within 280°C, so the preparation of pentacene film can be carried out. The purity of the pentacene powder used for preparation is 99% (purchased from TCL Technology Group Co., Ltd.), and its melting point is 372-374°C. Use a dust-free cotton swab dipped in anhydrous ethanol to clean the surface of the diamond anvil under a microscope to ensure that there is no debris on the surface that does not affect the deposition of the pentacene film. Invert the cleaned diamond anvil on the annular base support, and pentacene will be deposited on the surface of the diamond anvil later.
[0081] Step 2: Seal the tubular channel, check the air tightness, turn on the gas flow meter, and introduce nitrogen to completely exhaust the air in the system. Weigh 10 mg of pentacene powder into a reflux quartz tube, and then place the quartz tube and pentacene powder into the heating area of the tubular channel.
[0082] Step 3: Place the cleaned diamond anvil on the base support, and place the base support at the far end of the heating zone. After heating and evaporation, pentacene is deposited here. Figure 1 Seal the whole system, check its air tightness, set the nitrogen flow rate to 50ml / min, and exhaust the air after 10 minutes.
[0083] Step 4: Set up the tubular channel heating program, check the system and start the program to heat up the coating. Start heating from 25°C, increase the temperature by 5°C per minute, and heat to 280°C after 50 minutes. Heat at 280°C for 5 hours, stop working after heating, and wait for it to cool down to room temperature. When the system cools down naturally, stop nitrogen flow and take out the diamond anvil, and obtain a pentacene film on the surface of the diamond tip.
[0084] Since the film prepared through the above steps needs to be subsequently tested and characterized together with the diamond anvil substrate, and the diamond anvil substrate will interfere with the detection signal during the detection process, Figure 4 As shown, half of the film on the diamond anvil base is erased to deduct the background signal in the subsequent experimental process. After pre-pressing the diamond anvil end with a T301 gasket, a sample cavity with a diameter of 500 microns is prepared by laser drilling. After the gasket is reset, the pressure-transmitting medium silicone oil and the standard pressure material ruby are directly added. After closing the two parts of the press and tightening the screws, a million-level atmospheric pressure can be achieved in the sample cavity. Static pressure is applied to the pentacene film on the diamond anvil. The schematic diagram of the sample cavity in the specific high-pressure test is shown in the figure. Figure 5 shown.
[0085] The steady-state absorption spectrum of the pentacene film on the diamond anvil cell substrate prepared by the above method is characterized. Figure 6 shown.
[0086] Example 2
[0087] The same method as in Example 1 was used to coat the pentacene material on a quartz glass substrate, and the prepared pentacene film was subjected to XRD testing. The test results are shown in FIG. Figure 7 As shown, the results show that the obtained pentacene film is polycrystalline, which is consistent with the diffraction peak of the pentacene film obtained by vacuum evaporation coating method (for details, see the literature: Tao Chunlan, Zhang Xuhui, Dong Maojun, et al. AFM and XRD study of pentacene film [J]. Functional Materials, 2007, (05): 740-742). In addition, the film was tested by scanning electron microscopy, and the results are as follows Figure 8 As shown, the surface undulation of the film is about 500nm, and the film distribution is relatively uniform.
[0088] Example 3
[0089] This embodiment uses the above device to prepare a rubrene film on a sapphire substrate, which specifically includes the following steps:
[0090] Step 1: Use a 800-micron table IIa diamond anvil (purchased from Shanghai Zhenyuan Material Technology Co., Ltd.) to conduct high-pressure experimental testing. Use a T301 stainless steel gasket for pre-compression and then perform laser drilling to prepare a sample cavity. The prepared sample cavity has a thickness of 200μm and a diameter of 500μm. The purity of the rubrene powder used for preparation is 99.5% (purchased from TCL Technology Group Co., Ltd.), and its melting point is 314°C. Use 50μm thick sapphire (purchased from Shenzhen Lanjingling Information Technology Co., Ltd.) as the substrate for coating. Place the cleaned sapphire upside down on the annular sample holder, and the rubrene will be deposited on the surface of the sapphire substrate later.
[0091] Step 2: Seal the tubular channel, check the air tightness, turn on the gas flow meter, and introduce nitrogen to completely exhaust the air in the system. Weigh 10 mg of rubrene powder into a reflux quartz tube, and then put the quartz tube and rubrene powder into the heating area of the tubular channel.
[0092] Step 3: Place the cleaned sapphire substrate on the substrate holder. The specific placement is as follows: Figure 3 As shown, the substrate is placed at the far end of the heating zone, and rubrene is heated and evaporated and deposited there, as shown in FIG. Figure 1 Seal the whole system, check its air tightness, set the nitrogen flow rate to 50ml / min, and exhaust the air after 10 minutes.
[0093] Step 4: Set the tubular channel heating program, the raw material zone heating temperature is 300°C, the heating rate is 5°C / min, the initial temperature is 25°C, and the temperature is raised to 300°C after one hour. Heating and evaporating at 300°C for 6 hours with a nitrogen flow rate of 200ml / min can prepare a rubrene film deposited on a sapphire substrate.
[0094] The rubrene film on the sapphire substrate prepared by the above method was subjected to XRD test and AFM characterization, and the results are as follows: Fig. 9 and Fig.10 As shown, the results show that the surface undulation of the rubrene film obtained by this preparation method is within 2nm, and the surface morphology is uniform and smooth. Compared with the powder raw material, the diffraction peaks of the film and the powder are obviously different, and the diffraction peak of the film is significantly less than the diffraction peak of the powder, which proves that the film prepared by this method has better crystallinity and good singleness.
[0095] The sapphire substrate coated with rubrene is broken, and the fragments of appropriate size are selected for high-pressure loading. The thickness of the sapphire substrate is 50μm, and the thickness of the rubrene film does not exceed 1μm. The thickness of the sample is less than the thickness of the sample cavity. It can be placed in the sample cavity and silicone oil and ruby can be added for high-pressure loading. The relative position of the sample and ruby in the sample cavity after loading under the microscope is shown as follows Fig.11As shown in Figure 2, the position of the sample in the sample chamber after loading is as follows: Fig.12 shown.
[0096] After high pressure loading, the film can be subjected to various optical characterization tests. The rubrene film prepared above is subjected to steady-state absorption spectroscopy characterization under different pressures in a high pressure chamber. The characterization results are as follows: Fig.13 As shown, the absorption curves of the raw materials are different under different pressures. Under high pressure, the electronic energy level of the film is changed, causing it to move toward the long wavelength region as a whole.
[0097] Comparative Example 1
[0098] This comparative example uses the above device to prepare a 6,13-bis(triisopropylsilylethynyl)pentacene film on a sapphire substrate. Specifically, the following steps are included:
[0099] Step 1: Weigh 20 mg of 6,13-bis(triisopropylsilylethynyl)pentacene powder into a reflux quartz tube, and then place the quartz tube and the raw material powder into the tubular channel heating area.
[0100] Step 2: Use sapphire with a thickness of 50 μm for coating, place the cleaned sapphire substrate on the substrate holder, and place the substrate holder at the far end of the heating zone, such as Figure 1 Seal the whole system, check its air tightness, set the nitrogen flow rate to 50ml / min, and exhaust the air after 10 minutes.
[0101] Step 3: Set the tubular channel heating program, the raw material zone heating temperature is 300°C, the heating rate is 5°C / min, the initial temperature is 25°C, and the temperature is increased to 300°C after one hour. Heat and evaporate at 300°C for 6 hours, and the nitrogen flow rate is 200ml / min.
[0102] After the system cooled naturally, it was found that no film was deposited on the sapphire substrate. The 6,13-bis(triisopropylsilylethynyl)pentacene powder in the reflux quartz tube melted during the heating process and solidified into a block solid after cooling. The reason may be that the melting point of 6,13-bis(triisopropylsilylethynyl)pentacene is low (276°C), it melts at high temperature without evaporation, and its molecular weight is large, so it is not easy to be carried by nitrogen and deposited as a film.
[0103] In summary, the thin film preparation device of the present application is suitable for coating of most small molecule compounds used to prepare organic semiconductor materials, and is particularly suitable for raw materials that are not soluble enough to be formed into films using a solution deposition method. In the actual preparation process, parameters such as the heating temperature, heating time, and gas flow rate can be adjusted according to the properties of different materials. The preparation method in the present application can replace the vacuum coating method to perform economical and high-quality sample film formation, and perform high-pressure experimental detection tests on the samples. For organic semiconductor material molecules with a low melting point and a large molecular weight, such as 6,13-bis(triisopropylsilylethynyl)pentacene in Comparative Example 1 of the present application, since it melts at high temperatures and is not easy to evaporate, it is more appropriate to use a solution deposition film formation method.
[0104] The above is only a preferred embodiment of the present invention, and is not any formal or substantial limitation of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and supplements without departing from the method of the present invention, and these improvements and supplements should also be regarded as the protection scope of the present invention. Any technician familiar with this profession, without departing from the spirit and scope of the present invention, can make some changes, modifications and evolutions of the technical content disclosed above, which are equivalent embodiments of the present invention; at the same time, any changes, modifications and evolutions of any equivalent changes made to the above embodiments based on the essential technology of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A device for preparing an organic semiconductor thin film, characterized in that: include: Tubular channels, material carriers, heating devices and gas pipelines; The gas pipeline is connected to the gas inlet end of the tubular channel; the raw material carrying device is located in the tubular channel for carrying the raw material, and the heating device is used to heat the raw material.
2. The device for preparing an organic semiconductor thin film according to claim 1, characterized in that: The raw material carrying device is a quartz tube, and the aperture of the air inlet of the quartz tube is larger than the aperture of the air outlet.
3. The device for preparing an organic semiconductor thin film according to claim 1, characterized in that: The gas pipeline is provided with a gas flow meter; and / or, the gas pipeline is provided with a barometer; and / or, the gas pipeline is provided with a gas valve.
4. The device for preparing an organic semiconductor thin film according to claim 1, characterized in that: Furnace plugs for heat preservation are arranged at both ends of the tubular channel.
5. The device for preparing an organic semiconductor thin film according to claim 1, characterized in that: The preparation device further comprises a base support, which is arranged in the tubular channel and is located downstream of the raw material supporting device along the gas flow direction.
6. A method for preparing an organic semiconductor thin film using the device according to any one of claims 1 to 5, characterized in that: The steps include: 1) placing a substrate into a tubular channel, arranged downstream of the raw material supporting device, and placing the substrate into the raw material supporting device; 2) Inert gas is introduced from the gas pipeline to maintain an inert gas flow channel from the gas inlet end to the gas outlet end in the tubular channel, and a heating device is used to heat the raw material. After the raw material evaporates, it is carried by the inert gas and deposited on the substrate surface; 3) After the deposition is completed, the heating is stopped to obtain an organic semiconductor film on the surface of the substrate.
7. The method according to claim 6, characterized in that The raw material is a small molecule compound, an oligomer and a derivative thereof having a conjugated structure, preferably any one of thiophene, pyrrole, carbazole, aniline, fluorene and condensed ring aromatic hydrocarbons.
8. The method according to claim 7, characterized in that The condensed ring aromatic hydrocarbons are one or more selected from tetracene, pentacene, tetracene derivatives or pentacene derivatives.
9. The method according to claim 6, characterized in that The substrate is any one of metal foil, glass, silicon wafer, plastic, diamond and sapphire.
10. The method according to claim 6, characterized in that The uniformity of the organic semiconductor film is regulated by adjusting the flow rate of the inert gas; and / or the thickness of the organic semiconductor film is regulated by adjusting the deposition time.
11. The method according to claim 6, characterized in that The heating temperature is lower than the melting point of the raw material; and / or the nitrogen flow rate is 5 to 300 ml / min.
12. A method for screening raw materials for preparing organic semiconductor thin films using the device according to any one of claims 1 to 5.