Novel high-linearity nanowire channel device and preparation method thereof

By using n-type heavy doping technology of shuttle gate and nanowire channel in high electron mobility transistors, the problem of insufficient linearity of HEMT is solved, the linearity and transconductance peak of the device are improved, and the process flow is simplified. , improves the performance and production efficiency of the device.

CN118969832APending Publication Date: 2024-11-15XIDIAN UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411037730.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing high-electron mobility transistors (HEMTs) have insufficient linearity in high-frequency applications, resulting in a decrease in signal transmission quality, and device-level linearization technology is complex and costly.

Method used

Using a new nanowire channel device, by setting a shuttle gate on the AlGaN/AlN barrier layer and performing n-type heavy doping in the source access region of the nanowire channel, the gate-source electric field is reduced and electron mobility is improved. and linearity.

Benefits of technology

Higher linearity and transconductance peaks are achieved, avoiding the reduction of transconductance peaks in traditional HEMT structures, while simplifying the process flow and improving the performance and production efficiency of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969832A_ABST
    Figure CN118969832A_ABST
Patent Text Reader

Abstract

The novel high-linearity nanowire channel device structurally comprises a substrate layer, a GaN buffer layer and an AlGaN / AlN barrier layer which are sequentially stacked from bottom to top, a source electrode and a drain electrode are deposited at the two ends of the AlGaN / AlN barrier layer respectively, a fusiform grid electrode is deposited on the side, close to the source electrode, of the barrier layer, a plurality of nanowire channels are formed in the barrier layer, n-type heavy doping is formed in a source access region, and n-type heavy doping is formed in a drain access region. Depositing side walls on two sides of the fusiform grid; the method comprises a substrate layer, a buffer layer and a barrier layer which are stacked in sequence, source and drain electrodes are prepared at two ends of the barrier layer respectively; depositing a Si3N4 mask layer on the surface of the device; a plurality of strip-shaped mask layers arranged at intervals are formed between the source and the drain; the outline of the fusiform gate is developed after photoetching; the mask layer of the gate region is removed, the grooves arranged at intervals are exposed, and a Fin-HEMT structure is formed; fusiform grids are prepared on the grooves arranged at intervals; removing the mask layer on the surface of the device; a side wall is formed on the edge of the fusiform grid, and ion implantation is performed on the source access region to form n-type heavy doping; the invention has the advantages of high linearity and simple process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of microelectronic technology, and in particular relates to a novel high-linearity nanowire channel device and a preparation method thereof. Background Art

[0002] High electron mobility transistors (HEMTs) are popular in high-frequency applications due to their high-density two-dimensional electron gas (2DEG) derived from gallium nitride (GaN)-based heterojunctions. With the development of wireless communication systems, networks need to provide higher data transmission rates, lower transmission delays, and higher signal quality, which requires high-performance electronic devices. Today, more and more GaN HEMTs are being used in radio frequency (RF) front ends to replace traditional silicon-based devices due to their excellent performance. In the RF front end, linearity is a key parameter in system design to ensure communication quality. Nonlinear problems can lead to output power saturation at high input power, increase the error vector amplitude, and further deteriorate the signal transmission quality.

[0003] The implementation of circuit-level linearization is becoming more and more complex and costly. Compared with circuit-level linearization technology, device-level linearization technology can avoid more complex circuits and higher energy consumption. Therefore, starting from the nonlinear physical mechanism at the device level, it has become a new research hotspot today. At present, a variety of physical mechanisms have been proposed to explain HEMT nonlinearity, such as source starvation, increased source drive resistance, photophonon scattering, interface scattering, trap effect, and self-heating effect. According to different physical mechanisms, researchers have successively proposed different optimization methods.

[0004] Joglekar et al. studied the transconductance (g m ) compensation technology (Joglekar S et al., "Large signal linearity enhancement of AlGaN / GaN high electron mobility transistors by device-level VT engineering for transconductance compensation," IEEE International Electron Devices Meeting (IEDM), pp. 25.3.1–25.3.4, 2017.), the core idea is to connect multiple devices with different threshold voltages in parallel along the gate width direction, which can effectively suppress the transconductance (g m ) to achieve higher linearity. Based on this, Zhang et al. prepared a new transconductance (g m) compensated HEMT (ZHANG K, KONG Y, ZHU G, et al. High-Linearity AlGaN / GaN FinFETs for Microwave Power Applications [J / OL]. IEEE Electron Device Letters, 2017, 38(5): 615-618. DOI: 10.1109 / LED.2017.2687440.), whose T-type gate has a wide middle and narrow sides along the gate width direction. The output current peak value (I d,max ) is 1735mA / mm, and the peak transconductance (g m,max ) is 273mS / mm, and the gate voltage swing (G VS ) up to 5.5V. In addition, the transconductance (g m ) also shows that the new structure suppresses the nonlinear harmonic components. However, compared with the traditional HEMT structure, its transconductance peak (g m,max ) has been reduced.

[0005] As the gate voltage increases, the electric field between the gate and the source also increases. When the electric field is higher than 10kV / cm, the electron velocity begins to quasi-saturate, making the source drive resistance (R s ) will also increase, and the electron mobility will decrease. In response to this, researchers proposed a method of heavily doping the gate-source path (PALACIOS T, RAJAN S, CHAKRABORTY A, et al. Influence of the dynamic access resistance in the g / sub m / and f / sub T / linearity of AlGaN / GaN HEMTs[J / OL]. IEEE Transactions on Electron Devices, 2005, 52(10): 2117-2123. DOI: 10.1109 / TED.2005.856180.), which reduces the electric field between the gate and the source, so that the electrons do not reach quasi-saturation, and thus the source drive resistance (R s ) changes slowly, improving linearity. Summary of the invention

[0006] In order to overcome the above-mentioned deficiencies of the prior art, the present invention aims to provide a novel high-linearity nanowire channel device and a method for preparing the same, which can reduce the gate-source electric field, improve the electron mobility, and improve the linearity and transconductance peak (g m,max ), so that the device not only has a wide gate voltage swing (GVS ), its transconductance peak (g m,max ) will not be reduced relative to the traditional RF HEMT structure.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is:

[0008] A novel high-linearity nanowire channel device comprises a substrate layer 1, a GaN buffer layer 2 and an AlGaN / AlN barrier layer 3 which are stacked in sequence from bottom to top, a source electrode 4 and a drain electrode 5 are deposited at both ends of the AlGaN / AlN barrier layer 3, a shuttle-shaped gate 6 is deposited on the side of the AlGaN / AlN barrier layer 3 close to the source electrode 4, a plurality of nanowire channels 10 which are wide in the middle and narrow on both sides are arranged on the AlGaN / AlN barrier layer 3 along the gate width direction, the shuttle-shaped gate 6 surrounds the nanowire channel 10, ion implantation is performed in the source access region of the nanowire channel 10 to form n-type heavy doping 8, and sidewalls 7 are deposited on both sides of the shuttle-shaped gate 6.

[0009] The shuttle-shaped gate 6 is a shuttle-shaped Ni-Au gate of a Fin-HEMT structure with an average gate length of 250 nm.

[0010] A total of 50-70 nanowire channels 10 are arranged under the shuttle-shaped gate 6, and each nanowire channel 10 is spaced 15 nm apart.

[0011] The n-type heavily doped layer 8 has an implantation depth of 11-15 nm.

[0012] A method for preparing a novel high linearity nanowire channel device comprises the following steps:

[0013] Step 1, obtaining an epitaxial substrate, wherein the epitaxial substrate comprises a substrate layer 1, a GaN buffer layer 2 and an AlGaN / AlN barrier layer 3 stacked in sequence;

[0014] Step 2, preparing a source electrode 4 at one end of the AlGaN / AlN barrier layer 3, and preparing a drain electrode 5 at the other end of the AlGaN / AlN barrier layer 3;

[0015] Step 3: Deposit Si on the device surface 3 N 4 The mask layer is etched to form a plurality of spaced-apart strip-shaped Si electrodes between the source electrode 4 and the drain electrode 5. 3 N 4 mask layer;

[0016] Step 4: After photolithography, the outline of the shuttle gate is developed and the gate area not covered by Si is etched away. 3 N 4 An AlGaN / AlN barrier layer 3 covered by the mask layer;

[0017] Step 5: Remove the Si in the gate area 3 N 4 A mask layer is formed to expose the grooves arranged at intervals to form a Fin-HEMT structure;

[0018] Step 6, preparing a shuttle-shaped gate 6 on the grooves arranged at intervals by lift-off technology;

[0019] Step 7: Remove Si from the device surface 3 N 4 mask layer;

[0020] Step 8, forming a sidewall 7 at the edge of the shuttle-shaped gate 6, and performing ion implantation in the source access region to form an n-type heavy doping 8.

[0021] The specific method of step 2 is:

[0022] Step 2.1, photolithography of a source electrode region and a drain electrode region on the AlGaN / AlN barrier layer 3;

[0023] Step 2.2, evaporating an ohmic metal on the AlGaN / AlN barrier layer 3 in the source electrode region and the drain electrode region and on the photoresist outside the source electrode region and the drain electrode region to form a source electrode 4 and a drain electrode 5, stripping the device after the ohmic metal evaporation to remove the ohmic metal and the photoresist outside the source electrode 4 and the drain electrode 5, and then rinsing the device with ultrapure water and blowing it dry with nitrogen;

[0024] In step 2.3, the device after ohmic metal evaporation and stripping is placed in a rapid thermal annealing furnace for annealing to form an ohmic contact between the ohmic metal and the heterojunction channel.

[0025] The specific method of step 3 is:

[0026] Step 3.1, deposit a 50-60nm layer of Si on the device surface 3 N 4 mask layer;

[0027] Step 3.2: Except for the source electrode region and the drain electrode region, 3 N 4 The mask layer is photolithographically formed into grooves with different intervals to form a nanowire channel structure;

[0028] Step 3.3, using an ICP etching process to remove the Si between the nanowire channels 10 and in the source electrode region and the drain electrode region 3 N 4 Mask layer, forming several spaced-apart strips of Si 3 N 4 Mask layer.

[0029] The specific method of step 4 is:

[0030] Step 4.1, photolithography and developing a shuttle gate region on the device surface;

[0031] Step 4.2, etch away the gate area not covered by Si 3 N 4 The AlGaN / AlN barrier layer 3 is covered by the mask layer.

[0032] Compared with the prior art, the present invention has the following advantages:

[0033] 1) Since the shape of the prepared gate is shuttle-shaped instead of rectangular, there is no need to perform additional ion implantation of different doses under the gate to obtain different threshold voltages. Instead, the gate on each nanowire has a different gate length, and the devices are connected in parallel to achieve multi-threshold coupling of the device, thereby improving the linearity of the device.

[0034] 2) The present invention performs n-type heavy doping 8 in the source access region, which further reduces the electric field between the gate and the source compared to a simple nanowire structure, better limits the quasi-saturation of electrons, makes the source drive resistance increase more slowly, and further better optimizes the linearity of the device.

[0035] 3) The present invention uses a lift-off technique when depositing the shuttle-shaped gate 6, the source electrode 4 and the drain electrode 5, rather than traditional deposition, photolithography and etching, and the process is simple to implement.

[0036] In summary, the present invention has the advantages of high linearity and simple process by gradually changing the gate shape to a shuttle-shaped gate 6 and performing heavy doping in the source access region. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] FIG1 is a schematic diagram of the structure of a novel high linearity nanowire channel device of the present invention; wherein FIG1(a) is a cross-sectional view of a nanowire channel 10 of the present invention, and FIG1(b) is a cross-sectional view of a non-nanowire channel of the present invention.

[0038] Figure 2 It is a preparation flow chart of the present invention.

[0039] Among them, 1. substrate layer; 2. GaN buffer layer; 3. AlGaN / AlN barrier layer; 4. source electrode; 5. drain electrode; 6. shuttle gate; 7. sidewall; 8. n-type heavy doping; 9. Si 3 N 4 Mask layer; 10. Nanowire channel. DETAILED DESCRIPTION

[0040] 1, a novel high linearity nanowire channel device of the present invention comprises: a SiC substrate 1, a GaN buffer layer 2, an AlGaN / AlN barrier layer 3, a source electrode 4, a drain electrode 5, a shuttle gate 6, a sidewall 7, an n-type heavily doped 8 and a Si3 N 4 Mask layer; wherein, a substrate layer 1, a GaN buffer layer 2 and an AlGaN / AlN barrier layer 3 are stacked in sequence from bottom to top, a source electrode 4 and a drain electrode 5 are deposited at both ends of the AlGaN / AlN barrier layer 3, a shuttle-shaped gate 6 is deposited on the side of the AlGaN / AlN barrier layer 3 close to the source electrode 4, a plurality of nanowire channels 10 with a wide middle and narrow sides are arranged on the AlGaN / AlN barrier layer 3 along the gate width direction, the shuttle-shaped gate 6 surrounds the nanowire channel 10, ion implantation is performed in the source access region of the nanowire channel 10 to form n-type heavy doping 8, and sidewalls 7 are deposited on both sides of the shuttle-shaped gate 6.

[0041] The GaN buffer layer 2 is an unintentionally doped layer of 1.8 to 2 μm; the AlGaN / AlN barrier layer 3 is 10 nm AlGaN and 1 nm AlN; the shuttle gate 6 is a shuttle Ni-Au gate of a Fin-HEMT structure with an average gate length of 250 nm, and the gate in the non-nanowire channel region just cuts off the two-dimensional electron gas (2DEG). A total of 50 nanowire channels 10 are arranged under the shuttle gate 6, and each nanowire channel 10 is spaced 15 nm apart; the sidewall 7 medium is SiO 2 The n-type heavily doped electrode 8 is close to the source electrode 4, and phosphorus ions are implanted from the surface to the AlGaN / AlN / GaN interface multiple times. The n-type heavily doped electrode 8 has an implantation depth of 11-15nm and a doping concentration of 5×10 18 cm -3 ; The gate-source spacing is 1.5μm, and the gate-drain spacing is 2μm.

[0042] Reference Figure 2 The preparation method of the present invention is described by the following examples.

[0043] Example 1

[0044] A method for preparing a novel high linearity nanowire channel device comprises the following steps:

[0045] Step 1: Obtain an epitaxial substrate, which includes a substrate layer 1, a GaN buffer layer 2 and an AlGaN / AlN barrier layer 3 stacked in sequence, wherein the substrate layer 1 is a SiC substrate.

[0046] Step 2, preparing a source electrode 4 at one end of the AlGaN / AlN barrier layer 3, and preparing a drain electrode 5 at the other end of the AlGaN / AlN barrier layer 3;

[0047] Step 2.1, photolithography of a source electrode region and a drain electrode region on the AlGaN / AlN barrier layer 3;

[0048] The epitaxial substrate is placed on a hot plate at 200°C and baked for 5 minutes to remove moisture from the epitaxial substrate; then, the AlGaN / AlN barrier layer 3 is coated with glue, and the spinning speed is 2000 rpm, the spinning time is 40s, and the spinning thickness is 0.35μm, and the device is placed on a hot plate at 200°C and baked for 5 minutes; the device that has been coated and spun is placed in a photolithography machine for exposure, and the exposed device is placed in a developer to remove the photoresist, and then it is rinsed with ultrapure water and blown dry with nitrogen to form a source electrode region and a drain electrode region;

[0049] Step 2.2, evaporating the source electrode 4 and the drain electrode 5 on the AlGaN / AlN barrier layer 3 in the source electrode region and the drain electrode region and on the photoresist outside the source electrode region and the drain electrode region;

[0050] Place the device in the electron beam evaporation station and wait until the vacuum degree of the reaction chamber of the electron beam evaporation station reaches 2×10 -6 After 1000 MHz and 500 MHz, ohmic metal is evaporated on the AlGaN / AlN barrier layer 3 in the source electrode region and the drain electrode region and on the photoresist outside the source electrode region and the drain electrode region to form a source electrode 4 and a drain electrode 5. The ohmic metal is Ti / Al / Ni / Au from bottom to top. Then, the device after the ohmic metal evaporation is stripped to remove the ohmic metal and photoresist outside the source electrode 4 and the drain electrode 5, and then the device is rinsed with ultrapure water and blown dry with nitrogen.

[0051] Step 2.3, annealing treatment;

[0052] The device after ohmic metal evaporation and stripping is placed in a rapid thermal annealing furnace for annealing to form an ohmic contact between the ohmic metal and the heterojunction channel. The annealing process conditions are: the annealing atmosphere is N 2 , annealing temperature is 840℃, and annealing time is 60s.

[0053] Step 3: Deposit Si on the device surface 3 N 4 The mask layer is etched to form a plurality of spaced-apart strip-shaped Si electrodes between the source electrode 4 and the drain electrode 5. 3 N 4 mask layer;

[0054] Step 3.1, deposit a 50nm layer of Si on the device surface using plasma enhanced chemical vapor deposition (PECVD) 3 N 4 The mask layer is grown under the following process conditions: 2 O and SiH 4 As the reaction gas, the substrate temperature is 250°C, the reaction chamber pressure is 600mTorr, and the RF power is 22W;

[0055] Step 3.2, in Si 3 N 4 The mask layer (except the source electrode region and the drain electrode region) is photolithographically formed into grooves with different intervals to form a nanowire channel structure;

[0056] First, bake the device on a hot plate at 200°C for 5 minutes; then, apply and spin the photoresist at a spinning speed of 4000 rpm, and bake the device on a hot plate at 150°C for 1 minute; then, place the device in an electron beam EBL lithography machine for exposure; finally, place the exposed device in a developer for 60 seconds and rinse it with ultrapure water and blow it dry with nitrogen;

[0057] Step 3.3, using an ICP etching process to remove the Si between the nanowire channels 10 and in the source electrode region and the drain electrode region 3 N 4 Mask layer, forming several spaced-apart strips of Si 3 N 4 Mask layer; its etching conditions are: the reaction gas is CF 4 and O 2 , the reaction chamber pressure is 10 mTorr, the RF powers of the upper electrode and the lower electrode are 100 W and 10 W respectively, and the etching depth is 50 nm until the AlGaN / AlN barrier layer 3 is exposed.

[0058] Step 4: After photolithography, the outline of the shuttle gate is developed and the gate area not covered by Si is etched away. 3 N 4 An AlGaN / AlN barrier layer 3 covered by the mask layer;

[0059] Step 4.1, photolithography and developing a shuttle gate region on the device surface;

[0060] The device was placed on a hot plate at 200°C and baked for 5 minutes; then, photoresist was coated and spun, with a spinning speed of 2000 rpm, a spinning time of 40 seconds, and a spun thickness of 0.35 μm, and the device was placed on a hot plate at 200°C and baked for 5 minutes; the device after coating and spun was placed in a photolithography machine for exposure, and the exposed device was placed in a developer for overdevelopment;

[0061] Step 4.2, etch away the gate area not covered by Si 3 N 4 An AlGaN / AlN barrier layer 3 covered by the mask layer;

[0062] The gate area not covered by Si is etched by ICP process. 3 N 4AlGaN / AlN barrier layer 3 covered by mask layer; process conditions: reaction gas is Cl 2 and BCl 3 , the reaction chamber pressure is 10mTorr, the RF power of the upper electrode and the lower electrode are 100W and 10W respectively, and the etching depth is 30nm.

[0063] Step 5: Remove the Si in the gate area 3 N 4 A mask layer is formed to expose the grooves arranged at intervals to form a Fin-HEMT structure;

[0064] The Si in the gate area is etched using the ICP process. 3 N 4 Mask layer; process conditions: reaction gas is CF 4 and O 2 , the reaction chamber pressure is 10mTorr, and the RF powers of the upper electrode and the lower electrode are 100W and 10W respectively.

[0065] Step 6, preparing a shuttle gate 6 on the grooves arranged at intervals by lift-off technology, so that the nanowire device has different threshold voltages;

[0066] Evaporating a gate electrode 6 on the photoresist in the gate electrode region and outside the gate electrode region;

[0067] Place the device in the electron beam evaporation station and wait until the vacuum degree of the reaction chamber of the electron beam evaporation station reaches 2×10 -6 After 0.04075°, metal is evaporated on the gate electrode region and the photoresist outside the gate electrode region; then, the device after metal evaporation is stripped to remove the metal and photoresist outside the gate electrode 6, and then the device is rinsed with ultrapure water and blown dry with nitrogen.

[0068] Step 7: Remove Si from the device surface 3 N 4 mask layer;

[0069] The process conditions are: the reaction gas is CF 4 and O 2 , the reaction chamber pressure is 10mTorr, and the RF powers of the upper electrode and the lower electrode are 100W and 10W respectively.

[0070] Step 8, forming a sidewall 7 at the edge of the shuttle-shaped gate 6 to prevent gate breakdown, and performing ion implantation in the source access region to form n-type heavy doping 8;

[0071] Step 8.1, forming a sidewall 7 at the edge of the shuttle-shaped gate 6;

[0072] A layer of SiO was deposited on the device surface by plasma enhanced chemical vapor deposition (PECVD). 2, and then remove this layer of SiO by dry etching 2 When the shuttle gate 6 is exposed, the etching is stopped immediately, so that the sidewalls 7 are formed on both sides of the shuttle gate 6; the etching process conditions are: the reaction gas is CHF 3 , the reaction chamber pressure is 10mTorr;

[0073] Step 8.2, implanting phosphorus ions into the source access area;

[0074] Multiple phosphorus ion selective implantations were performed between the source electrode 4 and the sidewall 7, with an implantation depth of 11 nm and a doping concentration of 5×10 18 cm -3 .

[0075] Example 2

[0076] A method for preparing a novel high linearity nanowire channel device comprises the following steps:

[0077] Step 1: Obtain an epitaxial substrate, which includes a substrate layer 1, a GaN buffer layer 2 and an AlGaN / AlN barrier layer 3 stacked in sequence, wherein the substrate layer 1 is a SiC substrate.

[0078] Step 2, preparing a source electrode 4 at one end of the AlGaN / AlN barrier layer 3, and preparing a drain electrode 5 at the other end of the AlGaN / AlN barrier layer 3;

[0079] Step 2.1, photolithography of a source electrode region and a drain electrode region on the AlGaN / AlN barrier layer 3;

[0080] The epitaxial substrate was placed on a hot plate at 180°C and baked for 3 minutes to remove moisture from the epitaxial substrate; then, the AlGaN / AlN barrier layer 3 was coated with glue, and the spinning speed was 2000 rpm, the spinning time was 40s, the spinning thickness was 0.35μm, and the device was placed on a hot plate at 100°C and baked for 2 minutes; the device after the coating and spinning was placed in a photolithography machine for exposure, and the exposed device was placed in a developer to remove the photoresist, and then it was rinsed with isopropanol and dried with nitrogen to form a source electrode region and a drain electrode region;

[0081] Step 2.2, evaporating the source electrode 4 and the drain electrode 5 on the AlGaN / AlN barrier layer 3 in the source electrode region and the drain electrode region and on the photoresist outside the source electrode region and the drain electrode region;

[0082] Place the device in the electron beam evaporation station and wait until the vacuum degree of the reaction chamber of the electron beam evaporation station reaches 2×10 -6After 1000 MHz and 500 MHz, ohmic metal is evaporated on the AlGaN / AlN barrier layer 3 in the source electrode region and the drain electrode region and on the photoresist outside the source electrode region and the drain electrode region to form a source electrode 4 and a drain electrode 5. The ohmic metal is Ti / Al / Ni / Au from bottom to top. Then, the device after the ohmic metal evaporation is stripped to remove the ohmic metal and photoresist outside the source electrode 4 and the drain electrode 5, and then the device is rinsed with isopropyl alcohol and blown dry with nitrogen.

[0083] Step 2.3, annealing treatment;

[0084] The device after ohmic metal evaporation and stripping is placed in a rapid thermal annealing furnace for annealing to form an ohmic contact between the ohmic metal and the heterojunction channel. The annealing process conditions are: the annealing atmosphere is N 2 , annealing temperature is 800℃, and annealing time is 30s.

[0085] Step 3: Deposit Si on the device surface 3 N 4 The mask layer is etched to form a plurality of spaced-apart strip-shaped Si electrodes between the source electrode 4 and the drain electrode 5. 3 N 4 mask layer;

[0086] Step 3.1, deposit a 50nm layer of Si on the device surface using plasma enhanced chemical vapor deposition (PECVD) 3 N 4 The mask layer is grown under the following process conditions: 2 O and SiH 4 As the reaction gas, the substrate temperature is 250°C, the reaction chamber pressure is 600mTorr, and the RF power is 22W;

[0087] Step 3.2, in Si 3 N 4 The mask layer (except the source electrode region and the drain electrode region) is photolithographically formed into grooves with different intervals to form a nanowire channel structure;

[0088] First, bake the device on a hot plate at 180°C for 3 minutes; then, apply and spin the photoresist at a spinning speed of 4000 rpm, and bake the device on a hot plate at 100°C for 2 minutes; then, place the device in an electron beam EBL lithography machine for exposure; finally, place the exposed device in a developer for 40 seconds and rinse it with isopropanol and blow dry it with nitrogen;

[0089] Step 3.3, using an ICP etching process to remove the Si between the nanowire channels 10 and in the source electrode region and the drain electrode region 3 N 4Mask layer, forming several spaced-apart strips of Si 3 N 4 Mask layer; its etching conditions are: the reaction gas is CF 4 and O 2 The reaction chamber pressure is 100 mTorr, the RF powers of the upper electrode and the lower electrode are 100 W and 10 W respectively, and the etching depth is 50 nm until the AlGaN / AlN barrier layer 3 is exposed.

[0090] Step 4: After photolithography, the outline of the shuttle gate is developed and the gate area not covered by Si is etched away. 3 N 4 An AlGaN / AlN barrier layer 3 covered by the mask layer;

[0091] Step 4.1, photolithography and developing a shuttle gate region on the device surface;

[0092] The device was placed on a hot plate at 180°C and baked for 3 minutes; then, photoresist was coated and spun, with a spinning speed of 2000 rpm, a spinning time of 40 seconds, and a spinning thickness of 0.35 μm, and the device was placed on a hot plate at 100°C and baked for 2 minutes; the device after coating and spun was placed in a photolithography machine for exposure, and the exposed device was placed in a developer for overdevelopment, and after development, the device was placed on a hot plate at 110°C and baked for 2 minutes;

[0093] Step 4.2, etch away the gate area not covered by Si 3 N 4 An AlGaN / AlN barrier layer 3 covered by the mask layer;

[0094] The gate area not covered by Si is etched by ICP process. 3 N 4 AlGaN / AlN barrier layer 3 covered by mask layer; process conditions: reaction gas is Cl 2 and BCl 3 , the reaction chamber pressure is 100mTorr, the RF power of the upper electrode and the lower electrode are 100W and 10W respectively, and the etching depth is 30nm.

[0095] Step 5: Remove the Si in the gate area 3 N 4 A mask layer is formed to expose the grooves arranged at intervals to form a Fin-HEMT structure;

[0096] The Si in the gate area is etched using the ICP process. 3 N 4 Mask layer; process conditions: reaction gas is CF 4 and O 2, the reaction chamber pressure is 100mTorr, and the RF powers of the upper electrode and the lower electrode are 100W and 10W, respectively.

[0097] Step 6, preparing a shuttle gate 6 on the grooves arranged at intervals by lift-off technology, so that the nanowire device has different threshold voltages;

[0098] Evaporating a gate electrode 6 on the photoresist in the gate electrode region and outside the gate electrode region;

[0099] Place the device in the electron beam evaporation station and wait until the vacuum degree of the reaction chamber of the electron beam evaporation station reaches 2×10 -6 After 0.5040 % Torr, metal is evaporated on the gate electrode region and the photoresist outside the gate electrode region; then, the device after metal evaporation is stripped to remove the metal and photoresist outside the gate electrode 6, and then the device is rinsed with isopropyl alcohol and blown dry with nitrogen.

[0100] Step 7: Remove Si from the device surface 3 N 4 mask layer;

[0101] The process conditions are: the reaction gas is CF 4 and O 2 , the reaction chamber pressure is 100mTorr, and the RF powers of the upper electrode and the lower electrode are 100W and 10W, respectively.

[0102] Step 8, forming a sidewall 7 at the edge of the shuttle-shaped gate 6 to prevent gate breakdown, and performing ion implantation in the source access region to form n-type heavy doping 8.

[0103] Step 8.1, forming a sidewall 7 at the edge of the shuttle-shaped gate 6;

[0104] A layer of SiO was deposited on the device surface by plasma enhanced chemical vapor deposition (PECVD). 2 , and then remove this layer of SiO by dry etching 2 When the shuttle gate 6 is exposed, the etching is stopped immediately, so that the sidewalls 7 are formed on both sides of the shuttle gate 6; the etching process conditions are: the reaction gas is CHF 3 , the reaction chamber pressure is 100mTorr;

[0105] Step 8.2, implanting phosphorus ions into the source access area;

[0106] Multiple phosphorus ion selective implantations were performed between the source electrode 4 and the sidewall 7, with an implantation depth of 13 nm and a doping concentration of 5×10 18 cm -3 .

[0107] Example 3

[0108] A method for preparing a novel high linearity nanowire channel device comprises the following steps:

[0109] Step 1: Obtain an epitaxial substrate, which includes a substrate layer 1, a GaN buffer layer 2 and an AlGaN / AlN barrier layer 3 stacked in sequence, wherein the substrate layer 1 is a SiC substrate.

[0110] Step 2, preparing a source electrode 4 at one end of the AlGaN / AlN barrier layer 3, and preparing a drain electrode 5 at the other end of the AlGaN / AlN barrier layer 3;

[0111] Step 2.1, photolithography of a source electrode region and a drain electrode region on the AlGaN / AlN barrier layer 3;

[0112] The epitaxial substrate was placed on a hot plate at 180°C and baked for 3 minutes to remove moisture from the epitaxial substrate. Then, the AlGaN / AlN barrier layer 3 was coated with glue, and the spinning speed was 4000 rpm, the spinning time was 20s, the spinning thickness was 0.35μm, and the device was placed on a hot plate at 100°C and baked for 2 minutes; the device that had been coated and spun was placed in a photolithography machine for exposure, and the exposed device was placed in a developer to remove the photoresist, and then rinsed with isopropanol and dried with nitrogen to form the source electrode region and the drain electrode region;

[0113] Step 2.2, evaporating the source electrode 4 and the drain electrode 5 on the AlGaN / AlN barrier layer 3 in the source electrode region and the drain electrode region and on the photoresist outside the source electrode region and the drain electrode region;

[0114] Place the device in the electron beam evaporation station and wait until the vacuum degree of the reaction chamber of the electron beam evaporation station reaches 2×10 -6 After 1000 MHz and 500 MHz, ohmic metal is evaporated on the AlGaN / AlN barrier layer 3 in the source electrode region and the drain electrode region and on the photoresist outside the source electrode region and the drain electrode region to form a source electrode 4 and a drain electrode 5. The ohmic metal is Ti / Al / Ni / Au from bottom to top. Then, the device after the ohmic metal evaporation is stripped to remove the ohmic metal and photoresist outside the source electrode 4 and the drain electrode 5, and then the device is rinsed with isopropyl alcohol and blown dry with nitrogen.

[0115] Step 2.3, annealing treatment;

[0116] The device after ohmic metal evaporation and stripping is placed in a rapid thermal annealing furnace for annealing to form an ohmic contact between the ohmic metal and the heterojunction channel. The annealing process conditions are: the annealing atmosphere is N 2 , annealing temperature is 810℃, and annealing time is 30s.

[0117] Step 3: Deposit Si on the device surface3 N 4 The mask layer is etched to form a plurality of spaced-apart strip-shaped Si electrodes between the source electrode 4 and the drain electrode 5. 3 N 4 mask layer;

[0118] Step 3.1: Deposit a 100nm layer of Si on the device surface using plasma enhanced chemical vapor deposition (PECVD). 3 N 4 The mask layer is grown under the following process conditions: 2 O and SiH 4 As the reaction gas, the substrate temperature is 250°C, the reaction chamber pressure is 600mTorr, and the RF power is 22W;

[0119] Step 3.2, in Si 3 N 4 The mask layer (except the source electrode region and the drain electrode region) is photolithographically formed into grooves with different intervals to form a nanowire channel structure;

[0120] First, bake the device on a hot plate at 180°C for 3 minutes; then, apply and spin the photoresist at a spinning speed of 4000 rpm, and bake the device on a hot plate at 100°C for 2 minutes; then, place the device in an electron beam EBL lithography machine for exposure; finally, place the exposed device in a developer for 40 seconds and rinse it with isopropanol and blow dry it with nitrogen;

[0121] Step 3.3, using an ICP etching process to remove the Si between the nanowire channels 10 and in the source electrode region and the drain electrode region 3 N 4 Mask layer, forming several spaced-apart strips of Si 3 N 4 Mask layer; its etching conditions are: the reaction gas is CF 4 and O 2 The reaction chamber pressure is 100 mTorr, the RF power of the upper electrode and the lower electrode is 100 W and 10 W respectively, and the etching depth is 100 nm until the AlGaN / AlN barrier layer 3 is exposed.

[0122] Step 4: After photolithography, the outline of the shuttle gate is developed and the gate area not covered by Si is etched away. 3 N 4 An AlGaN / AlN barrier layer 3 covered by the mask layer;

[0123] Step 4.1, photolithography and development of the shuttle gate region on the device surface.

[0124] The device was placed on a hot plate at 180°C and baked for 3 minutes; then, photoresist was coated and spun, with a spinning speed of 4000 rpm, a spinning time of 20 seconds, and a spinning thickness of 0.35 μm, and the device was placed on a hot plate at 100°C and baked for 2 minutes; the device after coating and spun was placed in a photolithography machine for exposure, and the exposed device was placed in a developer for overdevelopment, and after development, the device was placed on a hot plate at 110°C and baked for 2 minutes;

[0125] Step 4.2, etch away the gate area not covered by Si 3 N 4 An AlGaN / AlN barrier layer 3 covered by the mask layer;

[0126] The gate area not covered by Si is etched by ICP process. 3 N 4 AlGaN / AlN barrier layer 3 covered by mask layer; process conditions: reaction gas is Cl 2 and BCl 3 , the reaction chamber pressure is 100mTorr, the RF power of the upper electrode and the lower electrode are 100W and 10W respectively, and the etching depth is 30nm.

[0127] Step 5: Remove the Si in the gate area 3 N 4 A mask layer is formed to expose the grooves arranged at intervals to form a Fin-HEMT structure;

[0128] Use BOE solution to etch away the Si in the gate area 3 N 4 Mask layer.

[0129] Step 6, preparing a shuttle gate 6 on the grooves arranged at intervals by lift-off technology, so that the nanowire device has different threshold voltages;

[0130] Evaporating a gate electrode 6 on the photoresist in the gate electrode region and outside the gate electrode region;

[0131] Place the device in the electron beam evaporation station and wait until the vacuum degree of the reaction chamber of the electron beam evaporation station reaches 2×10 -6 After 0.5040 % Torr, metal is evaporated on the gate electrode region and the photoresist outside the gate electrode region; then, the device after metal evaporation is stripped to remove the metal and photoresist outside the gate electrode 6, and then the device is rinsed with isopropyl alcohol and blown dry with nitrogen.

[0132] Step 7: Remove Si from the device surface 3 N 4 mask layer;

[0133] The process conditions are: the reaction gas is CF 4 and O2 , the reaction chamber pressure is 100mTorr, and the RF powers of the upper electrode and the lower electrode are 100W and 10W, respectively.

[0134] Step 8, forming a sidewall 7 at the edge of the shuttle-shaped gate 6 to prevent gate breakdown, and performing ion implantation in the source access region to form n-type heavy doping 8;

[0135] Step 8.1, forming a sidewall 7 at the edge of the shuttle-shaped gate 6;

[0136] A layer of SiO was deposited on the device surface by plasma enhanced chemical vapor deposition (PECVD). 2 , and then remove this layer of SiO by dry etching 2 When the shuttle gate 6 is exposed, the etching is stopped immediately, so that the sidewalls 7 are formed on both sides of the shuttle gate 6; the etching process conditions are: the reaction gas is CHF 3 , the reaction chamber pressure is 100mTorr;

[0137] Step 8.2, implanting phosphorus ions into the source access area;

[0138] Multiple phosphorus ion selective implantations were performed between the source electrode 4 and the sidewall 7, with an implantation depth of 15 nm and a doping concentration of 6×10 18 cm -3 .

[0139] In summary, the present invention is based on the traditional nanowire device, and changes the gate shape into a shuttle shape, so that each nanowire channel has a different threshold voltage, and there is no need to perform ion implantation of different doses; in addition, n-type heavy doping 8 is performed in the source access region, which reduces the driving resistance (Rs) and electric field between the source and drain, making it difficult for the electron speed to reach quasi-saturation, and better improving the gate voltage swing (GVS) and transconductance peak (g m,max ), the device has better linearity.

Claims

1. A novel high linearity nanowire channel device, characterized in that: The invention comprises a substrate layer (1), a GaN buffer layer (2) and an AlGaN / AlN barrier layer (3) which are stacked in sequence from bottom to top; a source electrode (4) and a drain electrode (5) are deposited at both ends of the AlGaN / AlN barrier layer (3); a shuttle-shaped gate (6) is deposited on the side of the AlGaN / AlN barrier layer (3) close to the source electrode (4); a plurality of nanowire channels (10) which are wide in the middle and narrow on both sides are arranged on the AlGaN / AlN barrier layer (3) along the gate width direction; the shuttle-shaped gate (6) surrounds the nanowire channel (10); ions are implanted into the source access region of the nanowire channel (10) to form n-type heavy doping (8); and sidewalls (7) are deposited on both sides of the shuttle-shaped gate (6).

2. A novel high linearity nanowire channel device according to claim 1, characterized in that: The shuttle-shaped gate (6) is a shuttle-shaped Ni-Au gate of a Fin-HEMT structure with an average gate length of 250nm.

3. A novel high linearity nanowire channel device according to claim 1 or 2, characterized in that: A total of 50-70 nanowire channels (10) are arranged under the shuttle-shaped gate (6), and each nanowire channel (10) is spaced 15 nm apart.

4. The novel high linearity nanowire channel device according to claim 1, characterized in that: The n-type heavy doping (8) has an implantation depth of 11-15 nm.

5. A novel method for preparing a high linearity nanowire channel device, characterized in that: The following steps are involved: Step 1, obtaining an epitaxial substrate, wherein the epitaxial substrate comprises a substrate layer (1), a GaN buffer layer (2) and an AlGaN / AlN barrier layer (3) stacked in sequence; Step 2, preparing a source electrode (4) at one end of the AlGaN / AlN barrier layer (3), and preparing a drain electrode (5) at the other end of the AlGaN / AlN barrier layer (3); Step 3, depositing a Si3N4 mask layer on the surface of the device, and etching to form a plurality of strip-shaped Si3N4 mask layers arranged at intervals between the source electrode (4) and the drain electrode (5); Step 4, developing the outline of the shuttle gate after photolithography, and etching away the AlGaN / AlN barrier layer (3) in the gate region not covered by the Si3N4 mask layer; Step 5, removing the Si3N4 mask layer in the gate region to expose the grooves arranged at intervals to form a Fin-HEMT structure; Step 6, preparing a shuttle-shaped gate (6) on the grooves arranged at intervals by a lift-off technique; Step 7, removing the Si3N4 mask layer on the surface of the device; Step 8, forming a side wall (7) at the edge of the shuttle-shaped gate (6), and performing ion implantation in the source access region to form n-type heavy doping (8).

6. The method for preparing a novel high linearity nanowire channel device according to claim 5, characterized in that: The specific method of step 2 is: Step 2.1, photolithography a source electrode region and a drain electrode region on the AlGaN / AlN barrier layer (3); Step 2.2, evaporating an ohmic metal on the AlGaN / AlN barrier layer (3) in the source electrode region and the drain electrode region and on the photoresist outside the source electrode region and the drain electrode region to form a source electrode (4) and a drain electrode (5), stripping the device after the ohmic metal evaporation to remove the ohmic metal and the photoresist outside the source electrode (4) and the drain electrode (5), and then rinsing the device with ultrapure water and blowing it dry with nitrogen; In step 2.3, the device after ohmic metal evaporation and stripping is placed in a rapid thermal annealing furnace for annealing to form an ohmic contact between the ohmic metal and the heterojunction channel.

7. The method for preparing a novel high linearity nanowire channel device according to claim 5, characterized in that: The specific method of step 3 is: Step 3.1, depositing a 50-60 nm Si3N4 mask layer on the device surface; Step 3.2, except for the source electrode region and the drain electrode region, grooves with different intervals are photoetched on the Si3N4 mask layer to form a nanowire channel structure; Step 3.3, using an ICP etching process to remove the Si3N4 mask layer between the nanowire channels (10) and in the source electrode region and the drain electrode region, to form a plurality of strip-shaped Si3N4 mask layers arranged at intervals.

8. The method for preparing a novel high linearity nanowire channel device according to claim 5, characterized in that: The specific method of step 4 is: Step 4.1, photolithography and developing a shuttle gate region on the device surface; Step 4.2, etching away the AlGaN / AlN barrier layer 3 in the gate region that is not covered by the Si3N4 mask layer.