Preparation method and application of chlorine removal mineral functional material for tobacco planting soil
The mineral functional materials generated by coal gangue roasting activation and acid reaction absorb chloride ions in tobacco soil, solving the problem of excessive or low chloride ion content in soil, improving the quality and combustion performance of tobacco leaves, and realizing the resource Recycling and economic benefits.
Patent Information
- Application Number
- CN202411163773.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-19
AI Technical Summary
Too high or too low chloride content in tobacco planting will affect the combustion performance and taste of tobacco leaves. The existing removal methods are costly or have adverse effects on the soil, and there is a lack of effective solutions.
After calcining and activation of coal gangue, soaking in acid and reacting with NaHCO3 and Na2CO3 salt solution to form a functional material for chlorine removal of minerals in tobacco planting soil, used to adsorb chloride ions in the soil and regulating chloride ion concentration.
This method can effectively reduce the concentration of chloride ion in tobacco planting soil, improve the combustion performance and taste of tobacco leaves, and is simple to operate, and has good economic benefits.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of agricultural planting soil additives, and in particular relates to a preparation method and application of a tobacco planting soil chlorine removal mineral functional material. Background Art
[0002] Tobacco is an important economic crop in my country. It is widely planted in Yunnan, Henan, Hunan, Shandong, Gansu and other places. The planting area is about 1.4 million hm2. 2 . The growth and development of tobacco is inseparable from the soil. The yield, quality and style characteristics of tobacco leaves are closely related to the soil. my country has a vast tobacco-growing area and complex soil types. The chloride ion content in different soils varies greatly. The chlorine content in tobacco leaves will significantly affect the combustion performance and smoking taste of tobacco. Excessive chlorine content in tobacco leaves will lead to poor combustion performance of tobacco and easy flameout. In addition, chlorine participates in plant photosynthesis and is an important component of chloroplasts and photosynthetic reactions. It is also a component of enzyme activators. It can regulate cell osmotic pressure and stomatal movement, reduce a variety of fungal diseases in plants, and is the trace element with the highest demand in the entire development process of tobacco. It has a significant impact on the smoking taste of tobacco.
[0003] It is ideal for tobacco leaves to contain 0.3% to 0.7% chlorine. Under this chlorine content, the tobacco leaves are soft, elastic and oily, have good expansion, increased shredding rate, low breakage rate, and can coordinate the chemical composition of tobacco leaves well; when the chlorine content of tobacco leaves is below 0.3%, the leaves become thinner, dry and rough, with a high fragmentation rate and a low filament rate, and the chloride ion content is too low, the burning speed of the cigarette stick is too fast, which will also have an adverse effect on the smoking process; when the chlorine content is above 0.8%, the quality of tobacco leaves is significantly reduced, the color of tobacco leaves is mottled or dull, the texture is too loose, difficult to store, easy to mold, and poor in combustion. At the same time, it affects the metabolism of sugar compounds in the leaves, affects sucrose synthesis, and hinders photosynthesis, thereby reducing the yield and quality of tobacco leaves. When the chlorine content of tobacco leaves exceeds 1.0%, the combustibility is reduced, and there is a seaweed smell when smoking, which will reduce the fragrance and taste. When the chlorine content of tobacco leaves exceeds 2.0%, flameout will occur.
[0004] At present, there are few studies on the relevant technologies for removing chloride ions from soil. The main methods include controlled irrigation and scientific fertilization, soil replacement, chemical improvement, bioremediation, and electrochemical remediation. The application of irrigation water and chlorine-containing fertilizers are important factors affecting the chloride content in tobacco-growing soils. Reasonable control of irrigation water and the application of chlorine-containing fertilizers is an effective means to reduce the chloride ion content in tobacco-growing soils from the source. For high-chlorine tobacco-growing soils, soil replacement is the most direct method, that is, replacing contaminated soil with uncontaminated soil. Although this method is simple, it is costly and the contaminated soil needs to be treated later. The chemical improvement method uses chemical reactions to transform and remove chloride ions in the soil, including chemical oxidation / reduction, precipitation and other methods. Among them, the chemical oxidation / reduction method is to add oxidants or oxidants to the soil to change the structure of pollutants or reduce the toxicity or mobility of pollutants through oxidation reactions or reduction reactions. The chemical precipitation method is a method of removing chloride ions by generating precipitation with chloride ions and other ions. It has the advantages of simple operation and fast reaction, but the chemical agents added in this method may have adverse effects on the soil. Bioremediation is the use of the metabolic activities of microorganisms and plants to degrade and remove soil pollutants. Tobacco is a leaf-producing economic crop that is sensitive to chlorine. Therefore, the previous crop can be planted to absorb and degrade the chloride ions in the tobacco-growing soil, so that the chloride ion content in the tobacco-growing soil is within an appropriate range. In addition, the adsorption method can be used to exchange the guest anions with the interlayer anions in a specific medium, and the adsorbent can be mixed with the soil to achieve the purpose of adsorbing chloride ions. In a comprehensive comparison, the adsorption method can be used to mix the adsorbent with tobacco-growing soil or irrigation water to reduce the chloride ion content in the soil, thereby improving the quality of tobacco leaves. The raw materials are easy to obtain and the operation is simple. Summary of the invention
[0005] In order to control the chloride ion content in the soil, the present invention provides a preparation method and application of a tobacco-growing soil dechlorination mineral functional material. The first purpose of the present invention is to provide a tobacco-growing soil dechlorination mineral functional material extracted from coal gangue, which is used to control the soil chloride ion concentration and improve the combustion performance and smoking taste of tobacco; the second purpose of the present invention is to provide a preparation method of a tobacco-growing soil dechlorination mineral functional material extracted from coal gangue; the third purpose of the present invention is to provide an application of a tobacco-growing soil dechlorination mineral functional material extracted from coal gangue.
[0006] A method for preparing a tobacco-growing soil dechlorination mineral functional material comprises the following steps: (1) crushing and grinding the coal gangue, sieving it with a sieve, calcining and activating the sieved coal gangue powder in a muffle furnace, and cooling it to room temperature to obtain activated coal gangue powder; (2) soaking the activated gangue powder obtained in step (1) in acid, filtering to remove insoluble impurities, and obtaining a gangue leaching solution; (3) slowly adding the precipitant dropwise to the gangue leachate obtained in step (2), stirring and reacting until no precipitate is precipitated, pouring off the upper clear liquid, and heating the lower solid-liquid mixture in a water bath for reaction; naturally cooling and filtering, washing the solid product obtained by filtration with deionized water until it is neutral, and drying in an oven to obtain the desired mineral functional material.
[0007] Preferably, the crushing and grinding of the coal gangue in step (1) is specifically to grind the coal gangue into particles with a particle size not greater than 0.5 mm in a ball mill at a rotation speed of 200-400 r / min, and then pass the particles through a 35-100 mesh sieve.
[0008] Preferably, the calcination activation temperature in step (1) is 500-700° C., and the activation time is 2-3 hours.
[0009] Furthermore, the calcination activation temperature is 600° C. and the activation time is 2 to 3 h.
[0010] Preferably, the acid used in step (2) is one of hydrochloric acid or sulfuric acid, the pH value is controlled at 1.0-2.5 during the acid leaching process, and the acid leaching time is 2-3 h.
[0011] Preferably, the precipitant in step (3) is a mixed salt solution of NaHCO3 and Na2CO3, and the specific operation is to mix NaHCO3 and Na2CO3 in proportion to ensure that the pH of the mixed salt solution is maintained at 9.5-10.0; when the gangue leachate is mixed with the precipitant, the gangue leachate is evenly added dropwise to the continuously stirred precipitant at a rate of 2-4 mL / min, and the amount of precipitant added is more than twice the amount of metal substances in the gangue leachate.
[0012] Preferably, in step (3), the solid-liquid mixture is heated in a water bath at a temperature of 70-80°C, and the reaction time is 10-12 h.
[0013] Preferably, in step (3), the oven drying temperature is 90-100°C and the drying time is 10-12 h.
[0014] Application of a tobacco-growing soil chlorine removal mineral functional material in controlling the chlorine content of tobacco leaves.
[0015] Preferably, adding the above-mentioned mineral functional materials to tobacco-growing soil with high chlorine content or using them to filter irrigation water with high chlorine content can effectively reduce the concentration of free chloride ions in tobacco-growing soil and regulate the chloride ion content in tobacco leaves.
[0016] Furthermore, the obtained mineral functional material is added to the high chlorine content tobacco planting soil, mixed thoroughly, and the addition amount is 10-100 kg per mu of soil.
[0017] Furthermore, the obtained mineral functional material is used to filter high-chlorine irrigation water. Specifically, the mineral functional material is added to the high-chlorine irrigation water for full contact for 12 to 36 hours, and the added amount is 5 to 100 kg per ton of water.
[0018] The benefit effect of the present invention is that the functional material for removing chlorine from tobacco-growing soil prepared by using coal gangue can absorb chloride ions from tobacco-growing soil or irrigation water with high chloride content. The material can transfer excessive chloride ions in the soil to the material through a replacement reaction, thereby reducing the chloride ion concentration in the soil. It has a good prospect in recycling coal gangue resources and regulating the chloride ion concentration of tobacco leaves to improve the quality of tobacco leaves. DETAILED DESCRIPTION
[0019] The present invention is further described below in conjunction with the embodiments, but the present invention is not limited in any way. Any changes or substitutions made based on the teachings of the present invention belong to the protection scope of the present invention.
[0020] The test methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.
[0021] Example 1 100 g of coal gangue (total aluminum content 42.17 g) containing 42.17% aluminum was calcined and activated in a box-type temperature-controlled furnace, kept at 600 ° C for 2 h, and then cooled to room temperature; the activated coal gangue was leached with sulfuric acid for 2 h, and the pH was controlled to 1.5. After the reaction was completed, the solid-liquid separation was performed. 6.0 g NaHCO3 and 4.0 g Na2CO3 were dissolved in 100 mL deionized water to prepare a precipitant, and the mixed metal salt solution was uniformly added to the precipitant at a rate of 3 mL / min. After the precipitation was completed, the pH of the solution was adjusted to 10.0, and stirring was continued for 30 min. After standing, it was aged in a water bath at 75 ° C for 11 h, and then filtered and washed with deionized water until neutral. The filter cake obtained after filtration was placed in a 105 ° C oven and dried for 10 h to obtain a mineral functional material. The obtained material (20 g) was mixed with chloride-containing soil (200 g), and the soil extract was collected after standing for 30 days. The soil chloride content decreased by 46%.
[0022] Example 2 100 g of coal gangue (total aluminum content 34.58 g) containing 34.58% aluminum was calcined and activated in a box-type temperature-controlled furnace, kept at 650°C for 2.5 h, and then cooled to room temperature; the activated coal gangue was leached with hydrochloric acid for 2.5 h, and the pH was controlled to 2.0. After the reaction was completed, the solid-liquid separation was performed. 3.0 g NaHCO3 and 6.5 g Na2CO3 were dissolved in 100 mL deionized water to prepare a precipitant, and the mixed metal salt solution was uniformly added to the precipitant at a rate of 4 mL / min. After the precipitation was completed, the pH of the solution was adjusted to 9.5, and stirring was continued for 30 min. After standing, it was aged in a water bath at 80°C for 10 h, and then filtered and washed with deionized water until neutral. The filter cake obtained after filtration was placed in a 100°C oven and dried for 11 h to obtain a mineral functional material. The obtained material (20 g) was mixed with chloride-containing soil (100 g), and the soil extract was collected after standing for 45 days. The soil chloride content decreased by 48%.
[0023] Example 3 100 g of coal gangue (38.1 g in total) containing 38.1% aluminum was calcined and activated in a box-type temperature-controlled furnace, kept at 550°C for 2.5 h, and then cooled to room temperature; the activated coal gangue was leached with hydrochloric acid for 3 h, and the pH was controlled to 1.5. After the reaction was completed, the solid-liquid separation was performed. 3.0 g of NaHCO3 and 6.5 g of Na2CO3 were dissolved in 100 mL of deionized water to prepare a precipitant, and the mixed metal salt solution was uniformly added to the precipitant at a rate of 3.5 mL / min. After the precipitation was completed, the pH of the solution was adjusted to 9.5, and stirring was continued for 30 min. After standing, it was aged in a water bath at 80°C for 10 h, and then filtered and washed with deionized water until neutral. The filter cake obtained after filtration was placed in a 100°C oven and dried for 11 h to obtain a mineral functional material. The obtained material (20 g) was mixed with chlorinated irrigation water (1000 ml) and reacted for 24 h. The chlorine content in the water was detected to be reduced by 52%.
Claims
1. A method for preparing a tobacco-growing soil dechlorination mineral functional material, Features The following steps are involved: (1) crushing and grinding the coal gangue, sieving it with a sieve, calcining and activating the sieved coal gangue powder in a muffle furnace, and cooling it to room temperature to obtain activated coal gangue powder; (2) soaking the activated gangue powder obtained in step (1) in acid, filtering to remove insoluble impurities, and obtaining a gangue leaching solution; (3) slowly adding the precipitant dropwise to the gangue leachate obtained in step (2), stirring and reacting until no precipitate is precipitated, pouring off the upper clear liquid, and heating the lower solid-liquid mixture in a water bath for reaction; naturally cooling and filtering, washing the solid product obtained by filtration with deionized water until it is neutral, and drying in an oven to obtain the desired mineral functional material.
2. The method according to claim 1, Features The coal gangue crushing and grinding in step (1) is specifically to grind the coal gangue into particles with a particle size not greater than 0.5 mm by a ball mill at a rotation speed of 200-400 r / min, and then pass through a 35-100 mesh sieve.
3. The method according to claim 1, Features The calcination activation temperature in step (1) is 500-700°C, and the activation time is 2-3h.
4. The method according to claim 1, Features The acid used in step (2) is hydrochloric acid or sulfuric acid. During the acid leaching process, the pH is controlled at 1.0-2.5, and the acid leaching time is 2-3 h.
5. The method according to claim 1, Features The precipitant in step (3) is NaHCO 3 and Na 2 CO 3 Mix the salt solution, specifically by mixing NaHCO 3 and Na 2 CO 3 Mix in proportion to ensure that the pH of the mixed salt solution is maintained at 9.5~10.0; when the gangue leachate is mixed with the precipitant, the gangue leachate is evenly added to the continuously stirred precipitant at a rate of 2~4 mL / min, and the amount of precipitant added is more than twice the amount of metal substances in the gangue leachate.
6. The method according to claim 1, Features The solid-liquid mixture in step (3) is heated in a water bath at a temperature of 70-80°C and the reaction time is 10-12 h.
7. Use of the mineral functional material according to claims 1 to 6 in controlling the chlorine content of tobacco leaves.
8. The use according to claim 7, Features The application method is to add the obtained mineral functional material to high-chlorine tobacco soil, fully mix it, and the addition amount is 10-100 kg per mu of soil.
9. The use according to claim 7, Features The application method is to use the obtained mineral functional material to filter high-chlorine irrigation water, specifically, to add the mineral functional material to the high-chlorine irrigation water, fully contact for 12 to 36 hours, and the addition amount is 5 to 100 kg per ton of water.
Citation Information
Patent Citations
Method for extracting Al2O3 from coal gangue
CN105480996A
Preparation method and application of high-performance coal gangue-based catalytic material
CN115475633A
Method for preparing FeOOH modified coal gangue from red mud