Biodegradable plastic film composition and preparation method thereof

By combining bio-based modified composites and nanocomposites, combined with supercritical fluid foaming and twin-screw extrusion technology, biodegradable plastic films with high mechanical strength and good degradation performance are prepared, and the existing technology is solved The safety, environmental performance and resource dependence of plastic films achieve environmentally friendly and durable packaging solutions.

CN118978800APending Publication Date: 2024-11-19JIANGSU JUFURUI NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411338576.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing biodegradable plastic films have poor safety, poor environmental performance, strong dependence on oil resources, poor thermal stability and light resistance, and are difficult to degrade on their own, resulting in ecological and environmental pollution.

Method used

Using a combination of bio-based modified composite materials, nanocomposite materials, processing aids and initiators, PHBV materials are modified by supercritical fluid foaming method, and biodegradable plastic film is prepared in a twin-screw extruder to improve mechanical strength Compatibility with interface.

Benefits of technology

It improves the tensile strength, elongation and degradation rate of plastic film, meets the needs of durability and environmental protection, reduces water absorption, and improves physical properties.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a biodegradable plastic film composition. The biodegradable plastic film composition comprises the following raw materials: a bio-based modified composite material, a nano composite material, a processing aid and an initiator. Wherein the bio-based modified composite material comprises modified PHBV and PHA, the modified PHBV material is prepared by adopting a supercritical fluid foaming method, the nano composite material comprises nano CuO, nano ZnO and nano SiO2, and the variety and proportion of the raw materials of the plastic film are optimized, so that the interfacial compatibility of the plastic film is improved, and the mechanical strength of the plastic film is improved. According to the biodegradable plastic film prepared by the invention, the quality of the plastic film is improved, the tensile strength and the elongation at break are improved, and the biodegradable plastic film has good physical properties and good degradation rate and is an environment-friendly plastic film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of plastic film preparation, and in particular to a biodegradable plastic film composition and a preparation method thereof. Background Art

[0002] At present, biodegradable plastic films have the following problems: First, polyethylene (PE), polyvinyl chloride (PVC), and polyvinylidene chloride (PVDC) have serious social problems such as poor safety, poor environmental performance, and strong dependence on non-renewable petroleum resources, and are subject to more and more restrictions in the field of food packaging. Secondly, polyvinyl chloride has poor thermal stability and light resistance. It begins to decompose hydrogen chloride gas that is harmful to the human body above 100°C and exposed to sunlight for a long time. Plasticizers such as diester adipate (DEHA) used in polyvinyl chloride films belong to endocrine disrupting environmental hormone substances that can induce cancer; thirdly, plastic films are difficult to degrade by themselves when discarded in the natural environment, especially PE films, which take hundreds of years to degrade, causing serious "white pollution" to the ecological environment. The raw materials of plastic films come from petroleum, which is a non-renewable resource. The large-scale use of plastic films will aggravate the energy crisis. Therefore, finding bio-based food packaging films made of natural materials or biosynthetic materials is a step-by-step approach to achieving the requirements of pollution-free and traceless packaging waste. Summary of the invention

[0003] In view of this, the present invention provides a biodegradable plastic film composition and a preparation method thereof to solve the above problems.

[0004] The technical solution of the present invention is achieved in this way:

[0005] A biodegradable plastic film composition comprises the following raw materials in parts by weight: 80-90 parts of bio-based modified composite materials; 2-10 parts of nano-composite materials; 1-3 parts of processing aids; and 2-3 parts of initiators. The bio-based composite material is composed of modified PHBV and PHA in a weight ratio of 3-4:1-1.5.

[0006] Furthermore, the preparation method of the modified PHBV is:

[0007] S1. Dry PHBV, CE and TMP-6000 at 60-65°C for 5-5.5h respectively;

[0008] S2, mixing the dried PHBV, CE and TMP-6000, stirring to obtain a mixture;

[0009] S3, melting the mixture and making it into strips to obtain a strip intermediate product;

[0010] S4, preparing modified PHBV by supercritical fluid foaming method;

[0011] Furthermore, the mass ratio of PHBV, CE and TMP-6000 is 9.5-10:0.2-0.3:0.04-0.06.

[0012] Furthermore, the mixed material is melted, the melting time is 5-7 minutes, the temperature is 180-190° C., and the rotation speed is 55-60 r / min.

[0013] Furthermore, the supercritical fluid foaming method injects supercritical carbon dioxide into a high-pressure foaming kettle, soaks the strip intermediate product for 30-50 minutes, the temperature is 140-150°C, the pressure is 20-25MPa, the temperature is reduced to 120-130°C, maintained for 16-22 minutes, then releases the pressure, and the temperature is reduced to 15-25°C to obtain modified PHBV.

[0014] Furthermore, the nano-composite material comprises nano-CuO, nano-ZnO and nano-SiO2 in a weight ratio of 2-3:1-1.5:1-1.5, and the particle size of the nano-composite material is 10-30 nm.

[0015] Furthermore, the processing aid comprises polyethylene wax and zinc stearate in a mass ratio of 1-2:0.6-0.8, and the initiator is an ammonium persulfate or potassium persulfate solution with a mass concentration of 5-7%.

[0016] A biodegradable plastic film composition comprises the following preparation steps:

[0017] S1. Mix the modified PHBV and PHA, and gelatinize at 75-80° C. for 10-15 min to obtain a bio-based modified composite material;

[0018] S3, mixing the bio-based modified composite material, the nano-composite material, the processing aid and the initiator, and stirring at high speed at 80-90° C. for 15-25 minutes to obtain a mixed material;

[0019] S3, placing the mixed material in a twin-screw extruder, extruding it, hot-melting it at 170-190°C, extruding it into a blown film, cutting it, dividing it into rolls, and packaging it to obtain a finished product.

[0020] Furthermore, the main engine speed of the twin-screw extruder is 15-30 rpm, and the material pressure is 3.0-3.5 MPA; the traction speed of the blown film is 4.0-5.0 rpm, and the winding speed is 7.5-8.0 rpm.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] In the production process of the biodegradable plastic film of the present invention, the raw materials are prepared by using bio-based modified composites, nano-composite materials, processing aids and initiators, and the PHBV material in the bio-based modified composite material is modified and prepared by a supercritical fluid foaming method, so as to further improve the mechanical strength of the plastic film, and by using nano-composite materials including nano-CuO, nano-ZnO and nano-SiO2, and by optimizing the types and formulas of the raw materials in large quantities, the interfacial compatibility of the plastic film is improved, the interfacial compatibility of the plastic film is enhanced, and the tensile strength and elongation at break are improved. The preparation method of the present invention improves the quality of the biodegradable plastic film, improves the tensile strength, has good physical properties, and meets the requirements of durability and environmental protection at the same time. DETAILED DESCRIPTION

[0023] In order to better understand the technical content of the present invention, specific examples are provided below to further illustrate the present invention. The experimental methods used in the examples of the present invention are all conventional methods unless otherwise specified.

[0024] Unless otherwise specified, the materials, reagents, etc. used in the embodiments of the present invention can be obtained from commercial sources.

[0025] PHBV: full name, poly (3-hydroxybutyrate-co-3-hydroxyvalerate), the molar content of hydroxyvalerate is 2%; manufacturer: Ningbo Tianan Biological Co., Ltd.

[0026] CE: Full name, ethylene-glycidyl methacrylate copolymer; Manufacturer: Xingbeida (Beijing) Chemical Materials Co., Ltd.

[0027] TMP-6000: chain extender, epoxy equivalent is 300g / mg; manufacturer: Hangzhou Ximao New Material Technology Co., Ltd.

[0028] Elongation at break (%) = (stretched length - original length) / original length × 100%

[0029] Water absorption rate (%) = (wet weight - dry weight) / dry weight × 100%

[0030] Example 1

[0031] A method for preparing raw material modified PHBV in a biodegradable plastic film composition comprises the following steps:

[0032] Step (1): PHBV, CE and TMP-6000 in a mass ratio of 10:0.3:0.06 were dried at 60°C for 5.5h;

[0033] Step (2): mixing the dried PHBV, CE and TMP-6000, stirring to obtain a mixture;

[0034] Step (3): melting the mixture, melting time 7 min, temperature 180° C., rotation speed 60 r / min, making into a spline, to obtain a spline intermediate product;

[0035] Step (4): The modified PHBV is prepared by supercritical fluid foaming method. Supercritical carbon dioxide is injected into a high-pressure foaming reactor to soak the intermediate product of the sample strip for 0.6 h at a temperature of 140° C. and a pressure of 20 MPa. The temperature is lowered to 130° C. and maintained for 22 min. After the pressure is released, the temperature is lowered to 25° C. to obtain the modified PHBV.

[0036] A preparation step of a biodegradable plastic film composition comprises:

[0037] Step (1): mixing modified PHBV and PHA in a weight ratio of 4:1.5, and gelatinizing at 78° C. for 15 minutes to obtain a bio-based modified composite material;

[0038] Step (2): 80 parts of a bio-based modified composite material; 4 parts of a nano-composite material (nano-CuO, nano-ZnO and nano-SiO2 in a weight ratio of 3:1:1.5), wherein the particle size of the nano-composite material is 30 nm; 3 parts of a processing aid (polyethylene wax and zinc stearate in a weight ratio of 2:0.5); and 3 parts of an initiator (a potassium persulfate solution with a mass concentration of 7%) are mixed, and stirred at high speed at 90° C. for 15 minutes to obtain a mixed material;

[0039] Step (3): extruding the mixture in a twin-screw extruder, with the main engine speed of the twin-screw extruder being 30 rpm and the material pressure being 3.5 MPA, hot melting at 190° C., extruding and blowing the film, with the traction speed of the film blowing being 5.0 rpm, cutting, winding, and winding speed being 8.0 rpm, and packaging to obtain the finished product.

[0040] Example 2

[0041] A method for preparing raw material modified PHBV in a biodegradable plastic film composition comprises the following steps:

[0042] Step (1): PHBV, CE and TMP-6000 in a mass ratio of 10:0.2:0.04 were dried at 60°C for 5 h;

[0043] Step (2): mixing the dried PHBV, CE and TMP-6000, stirring to obtain a mixture;

[0044] Step (3): melting the mixture, melting time 5 min, temperature 180° C., rotation speed 55 r / min, making into a spline, to obtain a spline intermediate product;

[0045] Step (4): The modified PHBV is prepared by supercritical fluid foaming method. Supercritical carbon dioxide is injected into a high-pressure foaming reactor to soak the intermediate product of the sample strip for 0.5 h at a temperature of 140° C. and a pressure of 20 MPa. The temperature is lowered to 120° C. and maintained for 15 min. The pressure is released and the temperature is lowered to 15° C. to obtain the modified PHBV.

[0046] A preparation step of a biodegradable plastic film composition comprises:

[0047] Step (1): mixing modified PHBV and PHA in a weight ratio of 3:1, and gelatinizing at 75° C. for 10 minutes to obtain a bio-based modified composite material;

[0048] Step (2): 90 parts of bio-based modified composite material; 5 parts of nano-composite material (nano-CuO, nano-ZnO and nano-SiO2 in a weight ratio of 2:1:1), wherein the nano-composite material has a particle size of 15 nm; 3 parts of processing aid (polyethylene wax and zinc stearate in a weight ratio of 1:0.6); and 2 parts of initiator (ammonium persulfate in a mass concentration of 5%) are mixed, and stirred at high speed at 80° C. for 15 minutes to obtain a mixed material;

[0049] Step (3): extruding the mixture in a twin-screw extruder, with the main engine speed of the twin-screw extruder being 15 rpm and the material pressure being 3.0 MPA, hot melting at 170° C., extruding and blowing the film, with the traction speed of the film blowing being 4.0 rpm, and the speed of cutting, winding and winding being 7.5 rpm, and packaging to obtain the finished product.

[0050] Example 3

[0051] A method for preparing raw material modified PHBV in a biodegradable plastic film composition comprises the following steps:

[0052] Step (1): PHBV, CE and TMP-6000 in a mass ratio of 10:0.3:0.05 were dried at 60°C for 5 h;

[0053] Step (2): mixing the dried PHBV, CE and TMP-6000, stirring to obtain a mixture;

[0054] Step (3): melting the mixture for 6 min at a temperature of 180° C. and a rotation speed of 60 r / min to prepare a strip to obtain a strip intermediate product;

[0055] Step (4): The modified PHBV is prepared by supercritical fluid foaming method. Supercritical carbon dioxide is injected into a high-pressure foaming reactor to soak the intermediate product of the sample strip for 0.6 h at a temperature of 140° C. and a pressure of 23 MPa. The temperature is lowered to 125° C. and maintained for 20 min. After the pressure is released, the temperature is lowered to 20° C. to obtain the modified PHBV.

[0056] A preparation step of a biodegradable plastic film composition comprises:

[0057] Step (1): mixing modified PHBV and PHA in a weight ratio of 3.5:1, and gelatinizing at 80° C. for 15 minutes to obtain a bio-based modified composite material;

[0058] Step (2): 90 parts of a bio-based modified composite material; 6 parts of a nano-composite material (nano-CuO, nano-ZnO and nano-SiO2 in a weight ratio of 2.5:1.2:1), wherein the particle size of the nano-composite material is 20 nm; 2 parts of a processing aid (polyethylene wax and zinc stearate in a weight ratio of 1.5:0.7); and 2.5 parts of an initiator (ammonium persulfate in a mass concentration of 6%) are mixed, and the mixture is stirred at high speed at 85° C. for 20 minutes to obtain a mixed material;

[0059] Step (3): extruding the mixture in a twin-screw extruder, wherein the main engine speed of the twin-screw extruder is 20 rpm, the material pressure is 3.3 MPa, hot melting is performed at 180° C., extruding and blowing the film, the traction speed of the blowing film is 4.5 rpm, the cutting, winding and winding speed are 7.5 rpm, and packaging is performed to obtain the finished product.

[0060] Comparative Example 1

[0061] The main difference between Comparative Example 1 and Example 3 is that in the preparation method of the modified PHBV, the raw material TMP-6000 is removed in step (1). The other steps are the same as those in Example 3.

[0062] Comparative Example 2

[0063] The main difference between Comparative Example 1 and Example 3 is that in the preparation method of modified PHBV, the raw material CE is removed in step (1). The other steps are the same as those in Example 3.

[0064] Comparative Example 3

[0065] The main difference between Comparative Example 4 and Example 3 is that in the preparation step (1) of a biodegradable plastic film, "modified PHBV and PHA in a weight ratio of 3.5:1 are mixed, and gelatinized at 80°C for 15 minutes to obtain a bio-based modified composite material" is replaced by "modified PHBV and PHA in a weight ratio of 1:1 are mixed, and gelatinized at 80°C for 15 minutes to obtain a bio-based modified composite material", that is, the proportion of modified PHBV in the raw materials is reduced, and the other steps are the same as Example 3.

[0066] Comparative Example 4

[0067] The main difference between Comparative Example 3 and Example 3 is that in the preparation step (2) of a biodegradable plastic film, the nanocomposite material replaces "nano-CuO, nano-ZnO and nano-SiO2 in a weight ratio of 2.5:1.2:1" with "nano-CuO, nano-ZnO and nano-SiO2 in a weight ratio of 0.2:1.2:1", that is, the proportion of nano-CuO is reduced. The other steps are the same as those in Example 3.

[0068] Comparison

[0069] Commercially available degradable plastic film, manufacturer: Shenyang Lidelong Plastic Products Co., Ltd.

[0070] Test example

[0071] The product performance of the plastic films prepared by the methods of Examples 1-3, Comparative Examples 1-4 and the control plastic films was measured, wherein 3 samples of the products prepared by each method were taken, and a total of 24 samples were taken. The mechanical strength was measured with reference to the GB / T 1040.1-2018 standard. The tensile strength and elongation at break of the biodegradable plastic film prepared by the methods of Examples 1-3 were higher than those of Comparative Examples 1-4, and higher than those of commercially available biodegradable plastic films. At the same time, the degradation rate of the biodegradable plastic film prepared by the methods of Examples 1-3 ranged from 99.2% to 99.5%, which was higher than that of Comparative Examples 1-4 and higher than that of commercially available plastic films.

[0072] Table 1

[0073] Group Tensile strength(Mpa) Elongation at break (%) Example 1 37.5 561.3 Example 2 37.2 559.8 Example 3 37.5 560.4 Comparative Example 1 31.1 503.3 Comparative Example 2 32.0 500.6 Comparative Example 3 32.7 439.8 Comparative Example 4 30.4 499.7 Comparison 28.8 436.2

[0074] The water resistance of the plastic film is reflected by calculating its water absorption rate. The lower the water absorption rate, the better the water resistance. The test method of water absorption rate is: cut a plastic film with a size of 30cm×30cm, weigh it, place it in pure water and soak it completely, soak it for 20 hours at room temperature, take out the plastic film, wipe it dry with absorbent paper, and weigh it again. Do 3 parallel tests and take the average. The degradation of the plastic film is evaluated by calculating the degradation rate. The specific degradation effect detection refers to the GB / T19277.1-2011 standard. The experimental results show that the biodegradable plastic film prepared by the method of Examples 1-3 has a degradation rate ranging from 99.2% to 99.5%, which is higher than that of Comparative Examples 1-4 and higher than that of commercially available biodegradable plastic films. At the same time, the water absorption rate of the biodegradable plastic film prepared by the method of Examples 1-3 is lower than that of Comparative Examples 1-4 and lower than that of commercially available plastic films.

[0075] Table 2

[0076] Group Degradation rate (%) Water absorption (%) Example 1 99.2 25.1 Example 2 99.5 24.8 Example 3 99.4 25.0 Comparative Example 1 89.5 39.2 Comparative Example 2 85.6 36.4 Comparative Example 3 84.1 35.8 Comparative Example 4 81.9 34.4 Comparison 80.5 38.0

[0077] Test results: The present invention adopts bio-based modified composites, nano-composites, processing aids and initiators, and the PHBV material in the bio-based modified composite is modified and prepared by supercritical fluid foaming method, and a nano-composite composed of nano-CuO, nano-ZnO and nano-SiO2 is used. At the same time, the types and formulas of raw materials are optimized in large quantities, and the interfacial compatibility of the plastic film is improved, thereby improving its mechanical strength. After the raw materials of the modified PHBV material are adjusted in Comparative Example 1-2, the tensile strength and elongation at break of the plastic film are reduced, indicating that the modified PHBV material prepared by the raw materials, proportions and preparation methods of the present invention has better performance. At the same time, in the preparation method of the plastic film of the present invention, Comparative Examples 3-4 adjust the proportion of modified PHBV and PHA, and after adjusting the proportion of nano-composites, the tensile strength, elongation at break and degradation rate are all reduced, indicating that the biodegradable plastic film prepared by the raw materials and methods of the present invention reduces water absorption, improves physical properties and stability, and is biodegradable, and can meet the requirements of durability and environmental protection at the same time.

[0078] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A biodegradable plastic film composition, characterized in that: The invention comprises the following raw materials in parts by weight: 80-90 parts of bio-based modified composite material, 2-10 parts of nano-composite material, 1-3 parts of processing aid, and 2-3 parts of initiator. The bio-based composite material is composed of modified PHBV and PHA.

2. A biodegradable plastic film composition according to claim 1, characterized in that: The weight ratio of the modified PHBV to PHA is (3-4):(1-1.5).

3. The biodegradable plastic film composition according to claim 1, characterized in that: The preparation method of the modified PHBV includes the following: S1. Dry PHBV, CE and TMP-6000 at 60-65°C for 5-5.5h respectively; S2, mixing the dried PHBV, CE and TMP-6000, stirring to obtain a mixture; S3, melting the mixture and making it into strips to obtain a strip intermediate product; S4. The strip intermediate product is subjected to supercritical fluid foaming method to obtain modified PHBV.

4. A biodegradable plastic film composition according to claim 3, characterized in that: The mass ratio of PHBV, CE and TMP-6000 is 9.5-10:0.2-0.3:0.04-0.

06.

5. The biodegradable plastic film composition according to claim 3, characterized in that: The melting time of the mixed material is 5-7 minutes, the temperature is 180-190° C., and the rotation speed is 55-60 r / min.

6. The biodegradable plastic film composition according to claim 3, characterized in that: The supercritical fluid foaming method comprises injecting supercritical carbon dioxide into a high-pressure foaming kettle, soaking the sample intermediate product for 30-50 minutes, at a temperature of 140-150° C. and a pressure of 20-25 MPa, cooling to 120-130° C., maintaining the pressure for 16-22 minutes, and then releasing the pressure, and then cooling to 15-25° C. to obtain modified PHBV.

7. The biodegradable plastic film composition according to claim 1, characterized in that: The nano composite material comprises nano CuO, nano ZnO and nano SiO2 in a weight ratio of 2-3:1-1.5:1-1.5, and the particle size of the nano composite material is 10-30 nm.

8. The biodegradable plastic film composition according to claim 1, characterized in that: The processing aid comprises polyethylene wax and zinc stearate in a mass ratio of 1-2:0.6-0.8, and the initiator is an ammonium persulfate or potassium persulfate solution with a mass concentration of 5%-7%.

9. The method for preparing a biodegradable plastic film composition according to claim 1, characterized in that: The method comprises the following preparation steps: S1. Mix the modified PHBV and PHA, and gelatinize at 75-80° C. for 10-15 min to obtain a bio-based modified composite material; S3, mixing the bio-based modified composite material, the nano-composite material, the processing aid and the initiator, and stirring at 80-90° C. for 15-25 minutes to obtain a mixed material; S3, placing the mixed material in a twin-screw extruder, extruding it, hot-melting it at 170-190°C, extruding it into a blown film, cutting it, dividing it into rolls, and packaging it to obtain a finished product.

10. The method for preparing a biodegradable plastic film composition according to claim 9, characterized in that: The main engine speed of the twin-screw extruder is 15-30 rpm, and the material pressure is 0-3.5 MPa; the traction speed of the film blowing is 4.0-5.0 rpm, and the winding speed is 7.5-8.0 rpm.