Environment-friendly antibacterial heat dissipation powder coating and production method thereof
By combining the preparation of inorganic carriers and antibacterial additives, the antibacterial and heat dissipation properties of powder coatings are improved, solving the problem of insufficient performance of existing weather-resistant powder coatings and achieving an environmentally friendly antibacterial and heat dissipation effect.
Patent Information
- Application Number
- CN202411474570.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-22
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing weather-resistant powder coatings have poor antibacterial and heat dissipation properties, which affects their service life and quality.
An inorganic carrier is prepared by hydrothermal synthesis using raw materials such as hydroxyl polyester resin, isophorone diisocyanate, and mica powder. This carrier is then combined with coupling agents and modifiers to prepare an antibacterial additive, forming a crisscrossing three-dimensional antibacterial network structure that enhances antibacterial and heat dissipation performance.
The prepared powder coating has excellent antibacterial and heat dissipation properties, extending its service life and ensuring its quality. At the same time, it is free of volatile solvents and harmful heavy metals, making it highly environmentally friendly.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings, and in particular to an environmentally friendly antibacterial heat-dissipating powder coating and a production method thereof. Background Art
[0002] Powder coating is completely different from general coating. It exists in the state of fine powder. Since no solvent is used, it is called powder coating. The main features of powder coating are harmlessness, high efficiency, resource saving and environmental protection. It includes two categories: thermoplastic powder coating and thermosetting powder coating. Thermoplastic powder coating has poor coating appearance and poor adhesion to metal, so it is rarely used in the field of automotive painting. Automotive painting generally uses thermosetting powder coating. Thermosetting powder coating uses thermosetting synthetic resin as film-forming material. During the drying process, the resin first melts and then solidifies into a smooth and hard coating after chemical cross-linking. The appearance, mechanical properties and corrosion resistance of the paint film formed by this kind of coating can meet the requirements of automotive finishing.
[0003] A weather-resistant powder coating and a preparation method thereof are disclosed in the patent document with application number "CN202311285824.3", which relates to the technical field of powder coatings. The weather-resistant powder coating comprises 135-155 parts by weight of a binder, 3%-12% by weight of a curing agent of the binder, 0.3-0.6 parts by weight of benzoin, 0.5-1 parts by weight of a leveling agent, 1.2-2.5 parts by weight of a dispersant, and 30-50 parts by weight of a pigment and filler. Although the powder coating prepared according to this patent document has excellent weather resistance and wear resistance, its antibacterial and heat dissipation properties are relatively poor, which not only shortens its service life to a certain extent, but also affects its quality. Therefore, the present invention provides an environmentally friendly antibacterial and heat-dissipating powder coating and a production method thereof to solve the above-mentioned technical problems. Summary of the invention
[0004] The purpose of the present invention is to provide an environmentally friendly antibacterial heat dissipation powder coating and a production method thereof. The produced powder coating not only has excellent antibacterial properties, but also has excellent heat dissipation properties, which prolongs its service life to a certain extent and also effectively guarantees its quality. Furthermore, the powder coating produced by the present invention does not contain any volatile solvents and harmful heavy metals, and is relatively environmentally friendly.
[0005] To achieve the above object, the present invention provides the following technical solutions: An environmentally friendly antibacterial heat dissipation powder coating is composed of the following raw materials in parts by weight: 90 to 110 parts of hydroxy polyester resin, 2 to 3 parts of 2,3-propylene oxide methacrylate, 1.0 to 1.5 parts of hydrogenated castor oil, 6 to 10 parts of curing agent, 15 to 20 parts of filler, 3 to 5 parts of leveling agent, 1.5 to 2.5 parts of dispersant, 10 to 15 parts of pigment and 8 to 12 parts of antibacterial additive; Wherein, the model of the hydroxy polyester resin is any one of HyPer H102, H301, H302, and H402.
[0006] Furthermore, the curing agent is selected from any one of isophorone diisocyanate, hexamethylene diisocyanate and hexyl diisocyanate.
[0007] Furthermore, the filler is selected from any one of mica powder, barium sulfate, silicon carbide, quartz powder and talcum powder.
[0008] Furthermore, the leveling agent is any one of GLP588, GLP388, GLP599, and PV88 leveling agents.
[0009] Furthermore, the dispersant is any one of BYK-190, BYK-996, and VOK-DS 330 dispersants.
[0010] Furthermore, the pigment is selected from any one of titanium dioxide, cobalt blue, cobalt green, carbon black, red iron oxide, and yellow iron oxide.
[0011] Furthermore, the preparation method of the antibacterial additive comprises the following steps: Step 1, dissolving 2-methoxy-4-(2-propenyl)phenol in chloroform with a mass of 5 to 8 times that of 2-methoxy-4-(2-propenyl)phenol, and sequentially adding azobisisobutyronitrile with a molar amount of 2 to 4% of 2-methoxy-4-(2-propenyl)phenol and 0.6 to 0.8 times of N-bromosuccinimide, mixing and stirring evenly, heating to 50 to 60°C, and stirring and reacting under nitrogen protection for 8 to 12 hours; after the reaction is completed, rotary evaporating the resulting component, and the remaining liquid component is recorded as a modifier; Step 2: uniformly dispersing the inorganic carrier in the coupling agent hydrolyzate at a solid-liquid ratio of 10 to 30 mg / mL, and stirring the reaction at a temperature of 50 to 60° C. for 5 to 8 hours. After the reaction is completed, the resulting components are sequentially subjected to solid-liquid separation, washing and drying treatment, and the resulting modified inorganic carrier is stored for standby use; Step 3: Add the modified inorganic carrier into anhydrous ethanol at a solid-liquid ratio of 5 to 15 mg / mL, and then add 0.8 to 1.2% of the modifier by mass of anhydrous ethanol and 0.5 to 0.8% of 3-fluorocinnamaldehyde in turn, mix and stir evenly, and then keep stirring and react at a temperature of 40 to 60°C for 4 to 6 hours; after the reaction is completed, the resulting components are sequentially subjected to solid-liquid separation, washing and drying treatment, and the final product is an antibacterial additive.
[0012] Furthermore, the preparation method of the coupling agent hydrolyzate comprises the following steps: adding 3-aminopropyltriethoxysilane at a dosage ratio of 0.05 to 0.08 mol / L into an ethanol aqueous solution with a volume concentration of 80 to 90%, and then adding γ-glycidyloxypropyltrimethoxysilane with a molar amount of 0.4 to 0.6 times that of 3-aminopropyltriethoxysilane, mixing and stirring evenly, adjusting the pH to 4.5 to 4.8, and magnetically stirring for 30 to 40 minutes to obtain the coupling agent hydrolyzate.
[0013] Furthermore, the preparation method of the inorganic carrier comprises the following steps: The first step is to add zinc sulfate to 2-5 g / L of graphene oxide aqueous dispersion at a dosage ratio of 0.2-0.5 mol / L, stir mechanically to completely dissolve it, then add sodium tartrate with a molar amount of 8-12% of zinc sulfate, stir for 3-5 minutes, and then disperse by ultrasonic for 5-8 minutes; The second step is to add a 30-40% volume of a 0.3-0.8 mol / L carbonamide aqueous solution to the mixed components while stirring at 800-1500 r / min. After the dispersion is completed, keep the mixture in a hot water bath at 120-150°C for 30-40 hours. After the reaction is completed, cool the resulting components naturally to room temperature, and then centrifuge, wash and dry them in sequence to obtain an inorganic carrier.
[0014] A method for producing an environmentally friendly antibacterial heat-dissipating powder coating comprises the following steps: weighing each raw material according to the formula amount, and putting each raw material into a mixing device for high-speed mixing and stirring for 10 to 20 minutes; after the mixing and stirring is uniform, transferring the obtained mixture into a twin-screw extruder for melt extrusion, and the extruded material is successively tableted, cooled to room temperature, crushed, ground and passed through a 100 to 200 mesh sieve, and the final product is the environmentally friendly antibacterial heat-dissipating powder coating.
[0015] Compared with the prior art, the present invention has the following beneficial effects: 1. The present invention uses graphene oxide, zinc sulfate, sodium tartrate and carbonamide as raw materials, and adopts a hydrothermal synthesis method to prepare an inorganic carrier composed of graphene and nano zinc oxide. The surface of the prepared inorganic carrier has an alternating concave and convex "valley-peak" structure, and there is also a porous structure inside; furthermore, a considerable number of graphene heat dissipation belts are buried on its surface. Finally, under the coordinated cooperation of the peak-valley structure, the porous structure and the graphene heat dissipation belt, the prepared inorganic carrier has excellent heat dissipation performance.
[0016] 2. The inorganic carrier prepared by the present invention is uniformly dispersed in the coupling agent hydrolyzate, so that 3-aminopropyl triethoxysilane and γ-glycidyl ether oxypropyl trimethoxysilane are uniformly dispersed and attached to the surface of the inorganic carrier and its internal porous structure, and then 3-aminopropyl triethoxysilane and γ-glycidyl ether oxypropyl trimethoxysilane react with the relevant active groups on the surface of the inorganic carrier to form a bond, and finally a modified inorganic carrier is prepared. The prepared modified inorganic carrier is put into anhydrous ethanol, and then the modifier and 3-fluorocinnamaldehyde are added in sequence, mixed and stirred evenly, and then stirred and reacted under heat preservation. Under the "bridge" effect of 3-aminopropyl triethoxysilane and γ-glycidyl ether oxypropyl trimethoxysilane, the modifier and 3-fluorocinnamaldehyde react with the active groups on the surface of the modified inorganic carrier respectively, and finally a criss-crossed three-dimensional antibacterial network structure is formed on the surface of the modified inorganic carrier and its internal porous structure. The antibacterial additive has excellent antibacterial properties under the synergistic cooperation of nano zinc oxide and three-dimensional antibacterial network structure. The use of the raw material of powder coating can not only effectively improve its antibacterial properties and heat dissipation properties, but also ensure its grade and quality. Furthermore, the powder coating produced by the present invention does not contain any volatile solvents and harmful heavy metals, and is relatively environmentally friendly. DETAILED DESCRIPTION
[0017] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0018] Example 1 An environmentally friendly antibacterial heat dissipation powder coating, composed of the following raw materials in parts by weight: 90 parts of hydroxy polyester resin, 2 parts of 2,3-propylene oxide methacrylate, 1.0 parts of hydrogenated castor oil, 6 parts of isophorone diisocyanate, 15 parts of mica powder, 3 parts of GLP588 leveling agent, 1.5 parts of BYK-190 dispersant, 10 parts of titanium dioxide and 8 parts of antibacterial additives; The hydroxy polyester resin is selected from the hydroxy polyester resin model HyPer H102 produced by Wuhan Hyperbranched Resin Technology Co., Ltd.
[0019] The preparation method of the antibacterial additive comprises the following steps: Step 1, dissolving 2-methoxy-4-(2-propenyl)phenol in chloroform with a mass of 5 times that of 2-methoxy-4-(2-propenyl)phenol, and sequentially adding azobisisobutyronitrile with a molar amount of 2% of 2-methoxy-4-(2-propenyl)phenol and 0.6 times of N-bromosuccinimide, mixing and stirring evenly, heating to 50°C, and stirring and reacting for 8 hours under nitrogen protection; after the reaction is completed, rotary evaporating the resulting components, and the remaining liquid components are recorded as modifiers; Step 2: Disperse the inorganic carrier evenly in the coupling agent hydrolyzate at a solid-liquid ratio of 10 mg / mL, and stir the reaction at a temperature of 50°C for 5 hours. After the reaction is completed, perform solid-liquid separation, washing and drying treatment on the resulting components in turn, and store the modified inorganic carrier for standby use; Step 3: Add the modified inorganic carrier into anhydrous ethanol at a solid-liquid ratio of 5 mg / mL, and then add 0.8% of the modifier by mass of anhydrous ethanol and 0.5% of 3-fluorocinnamaldehyde in turn, mix and stir evenly, and then keep stirring and react at a temperature of 40°C for 4 hours; after the reaction is completed, perform solid-liquid separation, washing and drying on the obtained product components in turn, and the final product is an antibacterial additive.
[0020] The preparation method of the coupling agent hydrolyzate comprises the following steps: adding 3-aminopropyltriethoxysilane at a dosage ratio of 0.05 mol / L into an ethanol aqueous solution with a volume concentration of 80%, then adding γ-glycidyloxypropyltrimethoxysilane with a molar amount of 0.4 times that of 3-aminopropyltriethoxysilane, mixing and stirring evenly, adjusting the pH to 4.5, and magnetically stirring for 30 minutes to obtain the coupling agent hydrolyzate.
[0021] The preparation method of the inorganic carrier comprises the following steps: The first step is to add zinc sulfate to a 2 g / L graphene oxide aqueous dispersion at a dosage ratio of 0.2 mol / L, stir mechanically to completely dissolve it, then add sodium tartrate with a molar amount of 8% of zinc sulfate, stir for 3 minutes, and then disperse by ultrasonication for 5 minutes; The second step, after dispersion is completed, add 30% of the volume and 0.3 mol / L of carbonamide aqueous solution into the obtained mixed components while stirring at 800 r / min. After stirring and dispersion, keep the mixture in a hot water bath at 120°C for 30 hours. After the reaction is completed, naturally cool the obtained product components to room temperature, and then centrifuge, wash and dry them in sequence to obtain the inorganic carrier.
[0022] A method for producing an environmentally friendly antibacterial heat-dissipating powder coating comprises the following steps: weighing each raw material according to the formula amount, and putting each raw material into a mixing device for high-speed mixing and stirring for 10 minutes; after the mixing and stirring is uniform, transferring the obtained mixture into a twin-screw extruder for melt extrusion, and the extruded material is successively tableted, cooled to room temperature, crushed, ground and passed through a 100-mesh sieve, and the final product is the environmentally friendly antibacterial heat-dissipating powder coating.
[0023] Example 2 The production method of an environmentally friendly antibacterial heat dissipation powder coating provided in this embodiment is basically the same as that in Example 1, except that the specific composition of the raw materials used and the preparation method of the antibacterial additive are not completely the same. The specific composition of the raw materials used in this embodiment and the preparation method of the antibacterial additive are as follows: An environmentally friendly antibacterial heat dissipation powder coating, composed of the following raw materials in parts by weight: 100 parts of hydroxy polyester resin, 2.5 parts of 2,3-propylene oxide methacrylate, 1.5 parts of hydrogenated castor oil, 8 parts of hexamethylene diisocyanate, 20 parts of barium sulfate, 4 parts of GLP388 leveling agent, 2.0 parts of BYK-996 dispersant, 12 parts of cobalt blue and 10 parts of antibacterial additives; The hydroxy polyester resin is selected from the hydroxy polyester resin model HyPer H301 produced by Wuhan Hyperbranched Resin Technology Co., Ltd.
[0024] The preparation method of the antibacterial additive comprises the following steps: Step 1, dissolving 2-methoxy-4-(2-propenyl)phenol in chloroform with a mass of 6 times that of 2-methoxy-4-(2-propenyl)phenol, adding azobisisobutyronitrile with a molar amount of 3% of 2-methoxy-4-(2-propenyl)phenol and 0.7 times of N-bromosuccinimide, mixing and stirring evenly, heating to 55°C, and stirring and reacting for 10 hours under nitrogen protection; after the reaction is completed, the resulting component is rotary evaporated, and the remaining liquid component is recorded as a modifier; Step 2: Disperse the inorganic carrier evenly in the coupling agent hydrolyzate at a solid-liquid ratio of 20 mg / mL, and stir the reaction at a temperature of 55°C for 6 hours. After the reaction is completed, perform solid-liquid separation, washing and drying on the resulting components in turn, and store the modified inorganic carrier for standby use; Step 3: Add the modified inorganic carrier into anhydrous ethanol at a solid-liquid ratio of 10 mg / mL, and then add 1.0% of the modifier by mass of anhydrous ethanol and 0.6% of 3-fluorocinnamaldehyde in turn, mix and stir evenly, and then keep stirring and react at a temperature of 50°C for 5 hours; after the reaction is completed, perform solid-liquid separation, washing and drying on the obtained product components in turn, and the final product is an antibacterial additive.
[0025] The preparation method of the coupling agent hydrolyzate comprises the following steps: adding 3-aminopropyltriethoxysilane at a dosage ratio of 0.06 mol / L into an ethanol aqueous solution with a volume concentration of 85%, then adding γ-glycidyloxypropyltrimethoxysilane with a molar amount of 0.5 times that of 3-aminopropyltriethoxysilane, mixing and stirring evenly, adjusting the pH to 4.6, and magnetically stirring for 35 minutes to obtain the coupling agent hydrolyzate.
[0026] The preparation method of the inorganic carrier comprises the following steps: The first step is to add zinc sulfate to a 4 g / L graphene oxide aqueous dispersion at a dosage ratio of 0.3 mol / L, stir mechanically to completely dissolve it, then add sodium tartrate with a molar amount of 10% of zinc sulfate, stir for 5 minutes, and then disperse by ultrasonication for 5 minutes; The second step, after dispersion is completed, add 35% volume and 0.5 mol / L concentration of carbonamide aqueous solution to the obtained mixed components while stirring at 1200r / min. After stirring and dispersion, keep warm in a hot water bath at 130°C for 35 hours; after the reaction is completed, naturally cool the obtained product components to room temperature, and then centrifuge, wash and dry them in sequence to obtain the inorganic carrier.
[0027] Example 3 The production method of an environmentally friendly antibacterial heat dissipation powder coating provided in this embodiment is basically the same as that in Example 1, except that the specific composition of the raw materials used and the preparation method of the antibacterial additive are not completely the same. The specific composition of the raw materials used in this embodiment and the preparation method of the antibacterial additive are as follows: An environmentally friendly antibacterial heat dissipation powder coating, composed of the following raw materials in parts by weight: 110 parts of hydroxy polyester resin, 3 parts of 2,3-propylene oxide methacrylate, 1.5 parts of hydrogenated castor oil, 10 parts of hexyl diisocyanate, 20 parts of silicon carbide, 5 parts of GLP599 leveling agent, 2.5 parts of VOK-DS 330 dispersant, 15 parts of cobalt green and 12 parts of antibacterial additives; The hydroxy polyester resin is selected from the hydroxy polyester resin model HyPer H302 produced by Wuhan Hyperbranched Resin Technology Co., Ltd.
[0028] The preparation method of the antibacterial additive comprises the following steps: Step 1, dissolving 2-methoxy-4-(2-propenyl)phenol in chloroform with a mass of 8 times that of 2-methoxy-4-(2-propenyl)phenol, adding azobisisobutyronitrile with a molar amount of 4% of 2-methoxy-4-(2-propenyl)phenol and 0.8 times of N-bromosuccinimide, mixing and stirring evenly, heating to 60°C, and stirring and reacting for 12 hours under nitrogen protection; after the reaction is completed, the resulting component is rotary evaporated, and the remaining liquid component is recorded as a modifier; Step 2: Disperse the inorganic carrier evenly in the coupling agent hydrolyzate at a solid-liquid ratio of 30 mg / mL, and stir the reaction at 60°C for 8 hours. After the reaction is completed, perform solid-liquid separation, washing and drying on the resulting components in turn, and store the modified inorganic carrier for future use; Step 3: Add the modified inorganic carrier into anhydrous ethanol at a solid-liquid ratio of 15 mg / mL, and then add 1.2% of the modifier by mass of anhydrous ethanol and 0.8% of 3-fluorocinnamaldehyde in turn, mix and stir evenly, and then keep stirring and react at 60°C for 6 hours; after the reaction is completed, perform solid-liquid separation, washing and drying on the resulting components in turn, and the final product is an antibacterial additive.
[0029] The preparation method of the coupling agent hydrolyzate comprises the following steps: adding 3-aminopropyltriethoxysilane at a dosage ratio of 0.08 mol / L into an ethanol aqueous solution with a volume concentration of 90%, then adding γ-glycidyloxypropyltrimethoxysilane with a molar amount of 0.6 times that of 3-aminopropyltriethoxysilane, mixing and stirring evenly, adjusting the pH to 4.8, and magnetically stirring for 40 minutes to obtain the coupling agent hydrolyzate.
[0030] The preparation method of the inorganic carrier comprises the following steps: The first step is to add zinc sulfate to a 5 g / L graphene oxide aqueous dispersion at a dosage ratio of 0.5 mol / L, stir mechanically to completely dissolve it, then add sodium tartrate with a molar amount of 12% of zinc sulfate, stir for 5 minutes, and then disperse by ultrasonication for 8 minutes; The second step, after dispersion is completed, add 40% of the volume and 0.8 mol / L of carbonamide aqueous solution into the obtained mixed components while stirring at 1500r / min. After stirring and dispersion, keep the mixture in a hot water bath at 150°C for 40 hours. After the reaction is completed, naturally cool the obtained product components to room temperature, and then centrifuge, wash and dry them in sequence to obtain the inorganic carrier.
[0031] Comparative Example 1: The main difference between this example and Example 1 is that an equal amount of inorganic carrier is used to replace the antibacterial additive in this example.
[0032] Comparative Example 2: The main difference between this example and Example 1 is that an equal amount of a modifier is used in this example to replace 3-fluorocinnamaldehyde.
[0033] Comparative Example 3: The main difference between this example and Example 1 is that an equal amount of 3-fluorocinnamaldehyde is used instead of the modifier in this example; and the total amount of the modifier and 3-fluorocinnamaldehyde in this example is equal to the total amount of the modifier and 3-fluorocinnamaldehyde in Comparative Example 2.
[0034] Performance Testing The high temperature resistant powder coating samples produced in Examples 1 to 3 and Comparative Examples 1 to 3 were sprayed on a 20 watt LED to obtain a coating film (coating thickness of 80±0.5 μm), and then the light retention rate, water contact angle, adhesion and heat dissipation performance of the coating film were tested. The obtained data are recorded in the following table: 1. Water contact angle test: The water contact angle of each group of test sample coatings was tested using the method described in GB / T 30693-2014.
[0035] 2. Gloss retention rate test: The gloss retention rate of each group of test sample coatings was tested using the method described in GB / T14522-2008.
[0036] 3. Antibacterial performance test: The antibacterial performance of the coating of each group of test samples was tested according to GB / T21866-2008 standard.
[0037] Note: .
[0038] By comparing and analyzing the relevant data in the table, it can be seen that the powder coating produced by the present invention not only has excellent antibacterial properties, but also has excellent heat dissipation properties, which prolongs its service life to a certain extent and also effectively guarantees its quality. This shows that the environmentally friendly antibacterial heat dissipation powder coating and its production method provided by the present invention have a broader market prospect and are more suitable for promotion.
[0039] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0040] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. An environmentally friendly antibacterial heat dissipation powder coating, It is characterized in that The invention is composed of the following raw materials in parts by weight: 90 to 110 parts of hydroxy polyester resin, 2 to 3 parts of 2,3-propylene oxide methacrylate, 1.0 to 1.5 parts of hydrogenated castor oil, 6 to 10 parts of curing agent, 15 to 20 parts of filler, 3 to 5 parts of leveling agent, 1.5 to 2.5 parts of dispersant, 10 to 15 parts of pigment and 8 to 12 parts of antibacterial additive; Wherein, the model of the hydroxy polyester resin is any one of HyPer H102, H301, H302, and H402.
2. The environmentally friendly antibacterial heat dissipation powder coating according to claim 1, Features: The curing agent is selected from any one of isophorone diisocyanate, hexamethylene diisocyanate and hexyl diisocyanate.
3. The environmentally friendly antibacterial heat dissipation powder coating according to claim 1, Features: The filler is selected from any one of mica powder, barium sulfate, silicon carbide, quartz powder and talcum powder.
4. The environmentally friendly antibacterial heat dissipation powder coating according to claim 1, Features: The leveling agent is selected from any one of GLP588, GLP388, GLP599, and PV88 leveling agents.
5. The environmentally friendly antibacterial heat dissipation powder coating according to claim 1, Features: The dispersant is any one of BYK-190, BYK-996 and VOK-DS 330.
6. The environmentally friendly antibacterial heat dissipation powder coating according to claim 1, Features: The pigment is selected from any one of titanium dioxide, cobalt blue, cobalt green, carbon black, red iron oxide and yellow iron oxide.
7. The environmentally friendly antibacterial heat dissipation powder coating according to claim 1, It is characterized in that The preparation method of the antibacterial additive comprises the following steps: Step 1, dissolving 2-methoxy-4-(2-propenyl)phenol in chloroform with a mass of 5 to 8 times that of 2-methoxy-4-(2-propenyl)phenol, and sequentially adding azobisisobutyronitrile with a molar amount of 2 to 4% of 2-methoxy-4-(2-propenyl)phenol and 0.6 to 0.8 times of N-bromosuccinimide, mixing and stirring evenly, heating to 50 to 60°C, and stirring and reacting under nitrogen protection for 8 to 12 hours; after the reaction is completed, rotary evaporating the resulting component, and the remaining liquid component is recorded as a modifier; Step 2: uniformly dispersing the inorganic carrier in the coupling agent hydrolyzate at a solid-liquid ratio of 10 to 30 mg / mL, and stirring the reaction at a temperature of 50 to 60° C. for 5 to 8 hours. After the reaction is completed, the resulting components are sequentially subjected to solid-liquid separation, washing and drying treatment, and the resulting modified inorganic carrier is stored for standby use; Step 3: Add the modified inorganic carrier into anhydrous ethanol at a solid-liquid ratio of 5 to 15 mg / mL, and then add 0.8 to 1.2% of the modifier by mass of anhydrous ethanol and 0.5 to 0.8% of 3-fluorocinnamaldehyde in turn, mix and stir evenly, and then keep stirring and react at a temperature of 40 to 60°C for 4 to 6 hours; after the reaction is completed, the resulting components are sequentially subjected to solid-liquid separation, washing and drying treatment, and the final product is an antibacterial additive.
8. The environmentally friendly antibacterial heat dissipation powder coating according to claim 7, It is characterized in that The preparation method of the coupling agent hydrolyzate comprises the following steps: adding 3-aminopropyltriethoxysilane in a dosage ratio of 0.05 to 0.08 mol / L into an ethanol aqueous solution with a volume concentration of 80 to 90%, then adding γ-glycidyloxypropyltrimethoxysilane with a molar amount of 0.4 to 0.6 times that of 3-aminopropyltriethoxysilane, mixing and stirring evenly, adjusting the pH to 4.5 to 4.8, and magnetically stirring for 30 to 40 minutes to obtain the coupling agent hydrolyzate.
9. The environmentally friendly antibacterial heat dissipation powder coating according to claim 7, It is characterized in that The preparation method of the inorganic carrier comprises the following steps: The first step is to add zinc sulfate to 2-5 g / L of graphene oxide aqueous dispersion at a dosage ratio of 0.2-0.5 mol / L, stir mechanically to completely dissolve it, then add sodium tartrate with a molar amount of 8-12% of zinc sulfate, stir for 3-5 minutes, and then disperse by ultrasonic for 5-8 minutes; The second step is to add a 30-40% volume of a 0.3-0.8 mol / L carbonamide aqueous solution to the mixed components while stirring at 800-1500 r / min. After the dispersion is completed, keep the mixture in a hot water bath at 120-150°C for 30-40 hours. After the reaction is completed, cool the resulting components naturally to room temperature, and then centrifuge, wash and dry them in sequence to obtain an inorganic carrier.
10. A method for producing an environmentally friendly antibacterial heat dissipation powder coating according to any one of claims 1 to 9, It is characterized in that The method comprises the following steps: weighing each raw material according to the formula amount, and putting each raw material into a mixing device for high-speed mixing and stirring for 10 to 20 minutes; after the mixing and stirring is uniform, transferring the obtained mixture into a twin-screw extruder for melt extrusion, and the extruded material is successively tableted, cooled to room temperature, crushed, ground and passed through a 100 to 200 mesh sieve, and the final product is an environmentally friendly antibacterial heat dissipation powder coating.
Citation Information
Patent Citations
High-isolation high-heat-conduction condom and preparation method thereof
CN108219221A
Preparation method of inorganic-organic hybrid antibacterial agent with antibacterial and hydrophobic functions and application of antibacterial agent
CN109627492A
Preparation method of inorganic-multiple organic composite antibacterial agent and application thereof
CN111410771A
Antibacterial and antivirus powder coating and preparation process thereof
CN111978772A
Weather-resistant powder coating, coating and preparation method
CN116102908A