Galvanized sheet surface defect analysis method and device and storage medium
Through the surface defect analysis method of galvanized sheet, including sample pretreatment and multi-layer EBSD analysis, the problem of difficulty in analyzing surface defects of galvanized sheets in the prior art is solved, and efficient and accurate defect detection is achieved.
Patent Information
- Application Number
- CN202411055116.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-19
AI Technical Summary
The prior art is difficult to effectively analyze the surface defects of galvanized plates for automobiles, especially when the aluminum heterogeneous layer between the zinc layer and the iron matrix exists. Conventional EBSD technology is not suitable for zinc layer analysis, which makes it difficult to distinguish defects.
Provide a method for surface defect analysis of galvanized plates, including sample selection, pretreatment, surface morphology analysis with zinc layer, surface morphology analysis of zinc-de-layer, defect cross-section morphology analysis and defect surface EBSD analysis, using field emission electron microscope and EBSD technology comprehensively analyzes the different hierarchical structures of galvanized plates.
Achieve pollution-free, low cost of consumables, short time-consuming, high working efficiency and high test accuracy analysis, which can fully demonstrate the orientation distribution state of different levels, ensuring the cleanliness of the detection surface and the effectiveness of the test .
Smart Images

Figure CN118980702A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of surface defect analysis of galvanized sheet, and in particular to a method, device and storage medium for surface defect analysis of galvanized sheet. Background Art
[0002] In scientific research, some surface defects often occur in galvanized sheets for automobiles, and it is necessary to analyze the causes of the problems. Such defects are more obvious on large sheet coils, and it is difficult to distinguish them with the naked eye after cutting them into small pieces.
[0003] The thickness of the zinc layer of galvanized sheets for automobiles is 5-9 microns. There is also an aluminum heterogeneous layer between the zinc layer and the iron matrix. The EBSD (backscattered electron diffraction technology) preparation process of conventional steel matrix is not suitable for zinc layer EBSD analysis. How to perform defect analysis on the surface of galvanized sheets has become an urgent problem to be solved. Summary of the invention
[0004] In view of this, the present invention provides a galvanized sheet surface defect analysis method, device and storage medium.
[0005] Specifically, the present invention is achieved through the following technical solutions:
[0006] According to a first aspect of the present invention, a method for analyzing surface defects of a galvanized sheet is provided, the method comprising the steps of:
[0007] Select galvanized sheet samples;
[0008] Pre-treating the galvanized sheet sample;
[0009] Conducting surface morphology analysis of the zinc layer on the galvanized sheet sample;
[0010] Conducting surface morphology analysis of the zinc removal layer on the galvanized sheet sample;
[0011] Performing defect cross-sectional morphology analysis on the galvanized sheet sample;
[0012] The defect surface EBSD analysis was performed on the galvanized sheet sample.
[0013] Optionally, the selecting of galvanized sheet samples comprises the steps of:
[0014] Select the galvanized sheet sample with surface defects as the inspection sample;
[0015] Select the auxiliary protection galvanized sheet samples with normal surface.
[0016] Optionally, the pretreatment of the galvanized sheet sample comprises the steps of:
[0017] Cutting the galvanized sheet sample into a preset size;
[0018] Grinding and cleaning the galvanized sheet sample;
[0019] The galvanized sheet samples are marked with sample numbers.
[0020] Optionally, the surface morphology analysis of the zinc layer on the galvanized sheet sample comprises the steps of:
[0021] Cleaning the galvanized sheet sample with alcohol ultrasonic wave and then drying it;
[0022] Cleaning the inspection surface of the galvanized sheet sample using a cleaning tape;
[0023] Blowing the galvanized sheet sample with compressed air;
[0024] The galvanized sheet samples were compared in morphology using a field emission electron microscope.
[0025] Optionally, the surface morphology analysis of the zinc removal layer of the galvanized sheet sample comprises the steps of:
[0026] removing the zinc layer of the galvanized sheet sample;
[0027] Cleaning the galvanized sheet sample with alcohol ultrasonic wave and then drying it;
[0028] Cleaning the inspection surface of the galvanized sheet sample using a cleaning tape;
[0029] Blowing the galvanized sheet sample with compressed air;
[0030] The galvanized sheet samples were compared in morphology using a field emission electron microscope.
[0031] Optionally, the defect cross-sectional morphology analysis of the galvanized sheet sample comprises the steps of:
[0032] Fixing the inspection sample galvanized sheet sample and the auxiliary protection sample galvanized sheet sample in the galvanized sheet sample together; grinding the bottom of the galvanized sheet sample;
[0033] Grinding and polishing the inspection surface of the galvanized sheet sample of the inspection sample;
[0034] Disassembling the auxiliary protection sample galvanized sheet sample;
[0035] Cleaning the galvanized sheet sample with alcohol ultrasonic wave and then drying it;
[0036] Cleaning the inspection surface of the galvanized sheet sample using a cleaning tape;
[0037] Blowing the galvanized sheet sample with compressed air;
[0038] The galvanized sheet samples were compared in morphology using a field emission electron microscope.
[0039] Optionally, the EBSD analysis of the defect surface of the galvanized sheet sample comprises the steps of:
[0040] Cleaning the galvanized sheet sample;
[0041] Performing EBSD analysis on the outermost layer of the zinc layer of the galvanized sheet sample;
[0042] Vibration polishing is performed on the outermost surface of the zinc layer of the galvanized sheet sample;
[0043] Performing EBSD analysis on the inner layer of the zinc layer of the galvanized sheet sample;
[0044] Vibration polishing is performed on the inner surface of the zinc layer of the galvanized sheet sample;
[0045] Performing EBSD analysis on the heterogeneous layer of the galvanized sheet sample;
[0046] Vibration polishing is performed on the surface of the heterogeneous layer of the galvanized sheet sample;
[0047] The EBSD analysis was performed on the outermost layer of the iron matrix of the galvanized sheet sample.
[0048] A galvanized sheet surface defect analysis device, comprising:
[0049] Sample selection module, used to select galvanized sheet samples;
[0050] A pretreatment module, used for pretreatment of the galvanized sheet sample;
[0051] A zinc layer analysis module is used to analyze the surface morphology of the zinc layer of the galvanized sheet sample;
[0052] A zinc removal layer analysis module is used to analyze the surface morphology of the zinc removal layer of the galvanized sheet sample;
[0053] A cross-sectional analysis module, used for performing defect cross-sectional morphology analysis on the galvanized sheet sample;
[0054] The surface analysis module is used to perform EBSD analysis on the defect surface of the galvanized sheet sample.
[0055] According to a third aspect of the present invention, there is provided an electronic device, comprising a memory, a processor, and a computer program stored in the memory and executable on the processor, wherein the processor implements the steps of any of the aforementioned methods when executing the program.
[0056] According to a fourth aspect of the present invention, there is provided a storage medium having a computer program stored thereon, wherein the program, when executed by a processor, implements the steps of any one of the aforementioned methods.
[0057] The technical solution provided by the present invention brings at least the following beneficial effects:
[0058] The present application provides a galvanized sheet surface defect analysis method, device and storage medium which are pollution-free, have low consumables cost, less time consumption, high work efficiency, wide application range, high test accuracy, rigorous scheme design, and can comprehensively display the orientation distribution states at different levels, thus ensuring the cleanliness of the detection surface and the effectiveness of the test. BRIEF DESCRIPTION OF THE DRAWINGS
[0059] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0060] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or related technical descriptions are briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0061] Figure 1 A schematic diagram of a process for analyzing surface defects of a galvanized sheet provided by an embodiment of the present invention;
[0062] Figure 2 A schematic diagram of the structure of a galvanized sheet surface defect analysis device provided by an embodiment of the present invention;
[0063] Figure 3 A schematic diagram of the structure of an electronic device provided by an embodiment of the present invention;
[0064] Figure 4 A schematic diagram of the structure of a storage medium provided by an embodiment of the present invention. DETAILED DESCRIPTION
[0065] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0066] Figure 1 A schematic flow chart of a galvanized sheet surface defect analysis method applicable to an embodiment of the present invention is shown schematically.
[0067] See also Figure 1 The embodiment of the present invention provides a method for analyzing surface defects of a galvanized sheet. The method can be applied to electronic devices, such as PCs, servers, terminals, etc. The method may include the following steps:
[0068] S1: Select galvanized sheet samples;
[0069] Exemplarily, the selecting of galvanized sheet samples comprises the steps of:
[0070] Select the galvanized sheet sample with surface defects as the inspection sample;
[0071] Select the auxiliary protection galvanized sheet samples with normal surface.
[0072] In the embodiment of the present application, two batches of samples are selected, one batch is the inspection sample galvanized sheet samples with surface defects, and the other batch is the auxiliary protection sample galvanized sheet samples with normal surfaces.
[0073] S2: pre-treating the galvanized sheet sample;
[0074] Exemplarily, the pretreatment of the galvanized sheet sample comprises the steps of:
[0075] Cutting the galvanized sheet sample into a preset size;
[0076] Grinding and cleaning the galvanized sheet sample;
[0077] The galvanized sheet samples are marked with sample numbers.
[0078] In the embodiment of the present application, the galvanized sheet sample is processed into a size of 20*10*thickness (mm) by wire cutting, with the long side in the rolling direction. The processing burrs of all samples are polished clean with 150-200 mesh sandpaper, and the sample number is marked with a typing pen in advance to prevent the marker pen mark from falling off during the sample preparation process and causing sample confusion. The mark is put on the left side of the sample to facilitate the observation of the order of sample placement in the sample compartment at any time in CCD mode (the working mode adopted by the CCD sensor when capturing images).
[0079] S3: Analyzing the surface morphology of the zinc layer on the galvanized sheet sample;
[0080] Exemplarily, the surface morphology analysis of the zinc layer on the galvanized sheet sample comprises the following steps:
[0081] Cleaning the galvanized sheet sample with alcohol ultrasonic wave and then drying it;
[0082] Cleaning the inspection surface of the galvanized sheet sample using a cleaning tape;
[0083] Blowing the galvanized sheet sample with compressed air;
[0084] The galvanized sheet samples were compared in morphology using a field emission electron microscope.
[0085] In the embodiment of the present application, the sample is cleaned 3-5 times with alcohol ultrasonic cleaning, each time for 8-10 minutes. After completion, the sample detection surface is tilted more than 30°, and the sample detection surface is vigorously rinsed from top to bottom with an alcohol pointed spray bottle to ensure that the detection surface is absolutely clean. Then place the sample under a hair dryer and blow hot air for 10-20 seconds to ensure that the sample is dry. Use special cleaning tape to perform a final clean on the sample inspection surface to remove some tiny particles that have not been cleaned. Use compressed air to clean and blow the entire sample table where the sample is placed to ensure overall cleanliness. When using a field emission electron microscope to compare the morphology of galvanized sheet samples, the Thermo Fisher field emission electron microscope is in 15KV, spot 6.0-10.0, and ETD mode to observe the surface morphology contrast of the samples, and use normal samples and defective samples at the same magnification for morphology comparison to find differences; the Thermo Fisher field emission electron microscope is in 15KV, spot 6.0-10.0, and T1 mode to observe the surface composition contrast of the samples, and use normal samples and defective samples at the same magnification for surface composition comparison to find differences; the Thermo Fisher field emission electron microscope is in 20KV, spot 11.0-13.0, and T1 mode to perform EDS composition analysis on the surface. The three methods of point analysis, line analysis, and surface analysis of the energy spectrum can be combined to perform component detection and comparison at the defect, analyze the types and contents of component elements in the detection area, and find differences between samples.
[0086] S4: Analyzing the surface morphology of the zinc removal layer of the galvanized sheet sample;
[0087] Exemplarily, the surface morphology analysis of the zinc removal layer of the galvanized sheet sample comprises the steps of:
[0088] removing the zinc layer of the galvanized sheet sample;
[0089] Cleaning the galvanized sheet sample with alcohol ultrasonic wave and then drying it;
[0090] Cleaning the inspection surface of the galvanized sheet sample using a cleaning tape;
[0091] Blowing the galvanized sheet sample with compressed air;
[0092] The galvanized sheet samples were compared in morphology using a field emission electron microscope.
[0093] In the embodiment of the present application, the sample is placed in a beaker, a certain amount of dezincification liquid is poured in (the amount should be enough to completely cover the sample), and it is left to stand for a period of time until no small bubbles are generated on the surface of the sample. Use tweezers to gently flip it in the middle to prevent the samples from being too close to each other and not being completely immersed in the dezincification liquid, resulting in incomplete dezincification. (The dezincification liquid is made by mixing distilled water and hydrochloric acid in a volume ratio of 5:1, the concentration of hydrochloric acid is 30% to 37%, and 4% to 6% of the total mass of hexamethylenetetramine is added as a corrosion inhibitor.) When the sample is cleaned with alcohol ultrasonic cleaning, it is cleaned 3-5 times in total, each time for 8-10 minutes. After completion, the detection surface is tilted more than 30°, and the detection surface is vigorously rinsed from top to bottom with an alcohol pointed spray pot to ensure that the detection surface is absolutely clean. Then place the sample under a hair dryer and blow hot air for 10-20 seconds to ensure that the sample is dry. Use special cleaning tape to clean the sample inspection surface for the final time to stick off some tiny particles that have not been cleaned. Finally, use compressed air to clean and blow the entire sample table where the sample is placed to ensure overall cleanliness. When using field emission electron microscopy to compare the galvanized sheet samples, observe the surface morphology contrast of the sample in the Thermo Fisher field emission electron microscope at 15KV, spot 6.0-10.0, ETD mode, and use normal samples and defective samples for morphology comparison at the same magnification to find differences; observe the surface composition contrast of the sample in the Thermo Fisher field emission electron microscope at 15KV, spot 6.0-10.0, T1 mode, and use normal samples and defective samples for surface composition comparison at the same magnification to find differences; perform EDS composition analysis on the surface in the Thermo Fisher field emission electron microscope at 20KV, spot 11.0-13.0, T1 mode, and use a combination of three methods of energy spectrum point analysis, line analysis, and surface analysis to perform component detection and comparison at the defect, analyze the types and contents of component elements in the detection area, and find differences between samples.
[0094] S5: performing defect cross-sectional morphology analysis on the galvanized sheet sample;
[0095] Exemplarily, the defect cross-sectional morphology analysis of the galvanized sheet sample comprises the following steps:
[0096] Fixing the inspection sample galvanized sheet sample and the auxiliary protection sample galvanized sheet sample in the galvanized sheet sample together;
[0097] Grinding the bottom of the galvanized sheet sample;
[0098] Grinding and polishing the inspection surface of the galvanized sheet sample of the inspection sample;
[0099] Disassembling the auxiliary protection sample galvanized sheet sample;
[0100] Cleaning the galvanized sheet sample with alcohol ultrasonic wave and then drying it;
[0101] Cleaning the inspection surface of the galvanized sheet sample using a cleaning tape;
[0102] Blowing the galvanized sheet sample with compressed air;
[0103] The galvanized sheet samples were compared in morphology using a field emission electron microscope.
[0104] In the embodiment of the present application, the test sample galvanized sheet sample and the auxiliary protection sample are fixed together by an auxiliary fixture. The bottom of the test sample galvanized sheet sample is ground with 100-200, 500-600, 900-1000 mesh sandpaper in sequence, and then roughly polished to make the bottom surface roughness ≤Ra0.02μm, which is conducive to increasing the adhesion between the sample and the sample stage, facilitating the improvement of the conductivity of the sample, and ensuring the observation effect of the sample. Reducing the roughness is more conducive to bonding the sample to the sample stage with double-sided conductive adhesive, increasing the adhesion, improving the conductivity of the sample, reducing the charging effect of the sample during the analysis process, and improving the analysis effect. After pre-treating the sample, this protective grinding is started on the inspected edge. The grinding procedure is a normal metallographic sample preparation process: use 100-200, 500-600 mesh sandpaper for rough grinding; use 1000-1200 mesh sandpaper for fine grinding; rough polishing; fine polishing; water polishing (deionized water, to ensure that the sample surface is clean and free of dirt). After completion, tilt the test surface by more than 30°, and use an alcohol spray bottle to vigorously rinse the test surface from top to bottom. After removing the dirt on the side, carefully disassemble the fixture and remove the auxiliary protection sample. This eliminates sample preparation problems such as sample edge arc, damage, and contamination caused by the grinding process, and retains the original morphology of the tested edge (zinc layer) to a large extent. The positive effects of rough polishing and fine polishing are: to further remove the stress deformation layer generated during sample grinding and reduce the influence of the stress layer on the analysis of the test surface. The prepared sample is ultrasonically cleaned with industrial alcohol with a concentration of more than 95% for 2-3 times, each time for 5-6 minutes. In order to clean the sticky velvet, muddy water, polishing paste particles and other external contaminants introduced during the preparation process. First, tilt the test surface by more than 30°, and use an alcohol spray bottle to vigorously rinse the test surface from top to bottom. Then put the sample under a hair dryer, and blow hot air for 10s-20s with the test surface tilted by more than 30° to ensure that the sample is dry. Use special cleaning tape to clean the sample inspection surface for the final time, and stick off some tiny particles that have not been cleaned. Finally, use compressed air to clean and blow the entire sample table where the sample is placed to ensure overall cleanliness. When using a field emission electron microscope to compare the morphology of galvanized sheet samples, observe the cross-sectional morphology of the samples in the Thermo Fisher field emission electron microscope in 15KV, spot 6.0-10.0, T1 mode, measure the thickness of the zinc layer, and observe the morphology and uniformity of the zinc layer. Use normal samples and defective samples at the same magnification to compare the morphology and find differences; use the Thermo Fisher field emission electron microscope in 20KV, spot 11.0-13.0, ETD or T1 mode to analyze the composition of the cross-section surface. The three methods of point analysis, line analysis, and surface analysis of the energy spectrum can be combined to compare the composition of the defect, analyze the types and contents of the component elements in the detection area, and find differences between samples.
[0105] S6: Performing EBSD analysis on the defect surface of the galvanized sheet sample.
[0106] Exemplarily, the EBSD analysis of the defect surface of the galvanized sheet sample comprises the steps of:
[0107] Cleaning the galvanized sheet sample;
[0108] Performing EBSD analysis on the outermost layer of the zinc layer of the galvanized sheet sample;
[0109] Vibration polishing is performed on the outermost surface of the galvanized sheet sample;
[0110] Performing EBSD analysis on the inner layer of the zinc layer of the galvanized sheet sample;
[0111] Vibration polishing is performed on the inner surface of the galvanized sheet sample;
[0112] Performing EBSD analysis on the heterogeneous layer of the galvanized sheet sample;
[0113] Vibration polishing is performed on the surface of the heterogeneous layer of the galvanized sheet sample;
[0114] The EBSD analysis was performed on the outermost layer of the iron matrix of the galvanized sheet sample.
[0115] In the embodiment of the present application, in order to better study the orientation relationship between the zinc layer and the substrate, the EBSD analysis of the galvanized sheet surface is divided into four stages. The EBSD analysis test parameters are: electron microscope HV 20KV, spot 13.0-16.0, ETD mode, WD 15-20mm, step length 2μm, magnification 100X. The whole process is for the same sample, and different stages are done in sequence. The galvanized sheet has four structural layers in total. The process fully and accurately expresses the true information of each structural layer, so as to better find the root cause of the sample defects in depth.
[0116] The first stage is EBSD analysis of the outermost layer of the zinc layer: EBSD analysis is performed directly on the surface of the sample after cleaning. The cleaning process is the same as the alcohol ultrasonic cleaning, drying, cleaning tape cleaning and compressed air wiping steps in step S5. Characterize the surface microstructure and tissue state of the zinc layer. Compare the defective samples with the normal samples to find the differences.
[0117] The second stage is the EBSD analysis of the inner layer of the zinc layer: the sample surface is directly vibrated and polished for 180±5min, the roughness of the test surface is less than 0.05μm, there is no counterweight, and the vibration frequency is 60-70%. The cleaning process is the same as the alcohol ultrasonic cleaning, drying, cleaning tape cleaning and compressed air wiping steps in step S5. The EBSD test is performed to characterize the internal microstructure and organizational state of the zinc layer, and the defective samples are compared with the normal samples to find the differences.
[0118] The third stage is the EBSD analysis of the heterogeneous layer Fe2Al5: the sample surface is directly vibrated and polished for 120±5min, with 3 weights and a vibration frequency of 60-70%. The cleaning process is the same as the alcohol ultrasonic cleaning, drying, cleaning tape cleaning and compressed air wiping steps in step S5. The EBSD test is performed to characterize the microstructure and organizational state of the transition layer, and the defective samples are compared with the normal samples to find the differences.
[0119] The fourth stage is the EBSD analysis of the outermost layer of the iron matrix: the zinc layer is completely removed with a dezincification solution, and after cleaning, it is directly vibrated and polished for 60min±5min, without a counterweight, and the vibration frequency is 80-90%. The cleaning process is the same as the alcohol ultrasonic cleaning, drying, cleaning tape cleaning and compressed air wiping steps in step S5. The EBSD test is performed to characterize the microstructure and organizational state of the original surface of the substrate before coating, and the defective samples are compared with the normal samples to find the differences.
[0120] like Figure 2 The present application provides a galvanized sheet surface defect analysis device, comprising:
[0121] The sample selection module 10 is used to select galvanized sheet samples;
[0122] A pretreatment module 20, used for pretreatment of the galvanized sheet sample;
[0123] A zinc layer analysis module 30 is used to analyze the surface morphology of the zinc layer of the galvanized sheet sample;
[0124] A zinc removal layer analysis module 40 is used to analyze the surface morphology of the zinc removal layer of the galvanized sheet sample;
[0125] A cross-sectional analysis module 50 is used to perform defect cross-sectional morphology analysis on the galvanized sheet sample;
[0126] The surface analysis module 60 is used to perform EBSD analysis on the defect surface of the galvanized sheet sample.
[0127] The galvanized sheet surface defect analysis device provided in the present application can execute the galvanized sheet surface defect analysis method provided in the above steps.
[0128] It should be understood that the above specific embodiments of the present invention are only used to illustrate or explain the principles of the present invention, and do not constitute a limitation of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present invention should be included in the protection scope of the present invention. In addition, the appended claims of the present invention are intended to cover all changes and modifications that fall within the scope and boundaries of the appended claims, or the equivalent forms of such scope and boundaries.
[0129] Reference below Figure 3, which shows a schematic diagram of the structure of an electronic device 100 suitable for implementing the embodiment of the present disclosure. The electronic device in the embodiment of the present disclosure may include, but is not limited to, mobile terminals such as mobile phones, notebook computers, digital broadcast receivers, PDAs (personal digital assistants), PADs (tablet computers), PMPs (portable multimedia players), vehicle terminals (such as vehicle navigation terminals), etc., and fixed terminals such as digital TVs, desktop computers, etc. Figure 3 The electronic device shown is only an example and should not bring any limitation to the functions and scope of use of the embodiments of the present disclosure.
[0130] like Figure 3 As shown, the electronic device 100 may include a processing device (e.g., a central processing unit, a graphics processing unit, etc.) 101, which can perform various appropriate actions and processes according to a program stored in a read-only memory (ROM) 102 or a program loaded from a storage device 108 to a random access memory (RAM) 103. In the RAM 103, various programs and data required for the operation of the electronic device 100 are also stored. The processing device 101, the ROM 102, and the RAM 103 are connected to each other via a bus 104. An input / output (I / O) interface 105 is also connected to the bus 104.
[0131] Typically, the following devices may be connected to the I / O interface 105: an input device 106 including, for example, a touch screen, a touchpad, a keyboard, a mouse, an image sensor, a microphone, an accelerometer, a gyroscope, etc.; an output device 107 including, for example, a liquid crystal display (LCD), a speaker, a vibrator, etc.; a storage device 108 including, for example, a magnetic tape, a hard disk, etc.; and a communication device 109. The communication device 109 may allow the electronic device 100 to communicate with other devices wirelessly or by wire to exchange data. Although the electronic device 100 having various devices is shown in the figure, it should be understood that it is not required to implement or have all the devices shown. More or fewer devices may be implemented or have alternatively.
[0132] In particular, according to an embodiment of the present disclosure, the process described above with reference to the flowchart can be implemented as a computer software program. For example, an embodiment of the present disclosure includes a computer program product, which includes a computer program carried on a computer-readable medium, and the computer program contains program code for executing the method shown in the flowchart. In such an embodiment, the computer program can be downloaded and installed from the network through the communication device 109, or installed from the storage device 108, or installed from the ROM 102. When the computer program is executed by the processing device 101, the above-mentioned functions defined in the method of the embodiment of the present disclosure are executed.
[0133] Reference below Figure 4, which shows a structural schematic diagram of a computer-readable storage medium suitable for implementing an embodiment of the present disclosure, wherein the computer-readable storage medium stores a computer program, and when the computer program is executed by a processor, it can implement the galvanized sheet surface defect analysis method as described in any of the above.
[0134] The present application also provides a computer program product, which includes a computer program / computer executable instructions, and when the computer program / computer executable instructions are executed by a processor of an electronic device, the steps of any of the above-mentioned methods for analyzing surface defects of galvanized sheets are implemented.
[0135] The present application provides a galvanized sheet surface defect analysis method, device and storage medium which are pollution-free, have low consumables cost, less time consumption, high work efficiency, wide application range, high test accuracy, rigorous scheme design, and can comprehensively display the orientation distribution states at different levels, thus ensuring the cleanliness of the detection surface and the effectiveness of the test.
[0136] It should be noted that, in this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0137] The foregoing is merely a specific embodiment of the present invention, which enables those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features claimed herein.
Claims
1. A method for analyzing surface defects of a galvanized sheet, characterized in that: The method comprises the steps of: Select galvanized sheet samples; Pre-treating the galvanized sheet sample; Conducting surface morphology analysis of the zinc layer on the galvanized sheet sample; Conducting surface morphology analysis of the zinc removal layer on the galvanized sheet sample; Performing defect cross-sectional morphology analysis on the galvanized sheet sample; The defect surface EBSD analysis was performed on the galvanized sheet sample.
2. The method for analyzing surface defects of a galvanized sheet according to claim 1, characterized in that: The selection of galvanized sheet samples comprises the following steps: Select the galvanized sheet sample with surface defects as the inspection sample; Select the auxiliary protection galvanized sheet samples with normal surface.
3. The method for analyzing surface defects of a galvanized sheet according to claim 1, characterized in that: The pretreatment of the galvanized sheet sample comprises the following steps: Cutting the galvanized sheet sample into a preset size; Grinding and cleaning the galvanized sheet sample; The galvanized sheet samples are marked with sample numbers.
4. The method for analyzing surface defects of a galvanized sheet according to claim 1, characterized in that: The surface morphology analysis of the zinc layer on the galvanized sheet sample comprises the following steps: Cleaning the galvanized sheet sample with alcohol ultrasonic wave and then drying it; Cleaning the inspection surface of the galvanized sheet sample using a cleaning tape; Blowing the galvanized sheet sample with compressed air; The galvanized sheet samples were compared in morphology using a field emission electron microscope.
5. The method for analyzing surface defects of a galvanized sheet according to claim 1, characterized in that: The surface morphology analysis of the zinc removal layer of the galvanized sheet sample comprises the following steps: removing the zinc layer of the galvanized sheet sample; Cleaning the galvanized sheet sample with alcohol ultrasonic wave and then drying it; Cleaning the inspection surface of the galvanized sheet sample using a cleaning tape; Blowing the galvanized sheet sample with compressed air; The galvanized sheet samples were compared in morphology using a field emission electron microscope.
6. The method for analyzing surface defects of a galvanized sheet according to claim 1, characterized in that: The defect cross-sectional morphology analysis of the galvanized sheet sample comprises the following steps: Fixing the inspection sample galvanized sheet sample and the auxiliary protection sample galvanized sheet sample in the galvanized sheet sample together; Grinding the bottom of the galvanized sheet sample; Grinding and polishing the inspection surface of the galvanized sheet sample of the inspection sample; Disassembling the auxiliary protection sample galvanized sheet sample; Cleaning the galvanized sheet sample with alcohol ultrasonic wave and then drying it; Cleaning the inspection surface of the galvanized sheet sample using a cleaning tape; Blowing the galvanized sheet sample with compressed air; The galvanized sheet samples were compared in morphology using a field emission electron microscope.
7. The method for analyzing surface defects of a galvanized sheet according to claim 1, characterized in that: The EBSD analysis of the defect surface of the galvanized sheet sample comprises the following steps: Cleaning the galvanized sheet sample; Performing EBSD analysis on the outermost layer of the zinc layer of the galvanized sheet sample; Vibration polishing is performed on the outermost surface of the zinc layer of the galvanized sheet sample; Performing EBSD analysis on the inner layer of the zinc layer of the galvanized sheet sample; Vibration polishing is performed on the inner surface of the zinc layer of the galvanized sheet sample; Performing EBSD analysis on the heterogeneous layer of the galvanized sheet sample; Vibration polishing is performed on the surface of the heterogeneous layer of the galvanized sheet sample; The EBSD analysis was performed on the outermost layer of the iron matrix of the galvanized sheet sample.
8. A galvanized sheet surface defect analysis device, characterized in that: include: Sample selection module, used to select galvanized sheet samples; A pretreatment module, used for pretreatment of the galvanized sheet sample; A zinc layer analysis module is used to analyze the surface morphology of the zinc layer of the galvanized sheet sample; A zinc removal layer analysis module is used to analyze the surface morphology of the zinc removal layer of the galvanized sheet sample; A cross-sectional analysis module, used for performing defect cross-sectional morphology analysis on the galvanized sheet sample; The surface analysis module is used to perform EBSD analysis on the defect surface of the galvanized sheet sample.
9. An electronic device comprising a memory, a processor, and a computer program stored in the memory and executable on the processor, characterized in that: When the processor executes the program, the steps of the method according to any one of claims 1 to 7 are implemented.
10. A storage medium having a computer program stored thereon, characterized in that: When the program is executed by a processor, the steps of the method according to any one of claims 1 to 7 are implemented.