Ultrathin electrolyte membrane and preparation method and application thereof
The preparation of ultra-thin electrolyte membranes through electrospinning and chemical crosslinking technology solves the problems of swelling and thickness control of electrolyte membranes in the prior art, achieves high performance and stability, and is suitable for high-performance electrochemical devices.
Patent Information
- Application Number
- CN202411039973.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
AI Technical Summary
The prior art has problems with swelling, difficulty in thickness control, and insufficient stability and durability when preparing ultra-thin electrolyte membranes, which affects the performance and reliability of the battery.
Precursor polymer films with uniformly dispersed hydrophobic and hydrophilic networks were prepared by electrospinning technology, and limited swelling polymer films were prepared by in-situ chemical crosslinking technology, combining appropriate hydrophobic and hydrophilic polymer ratios and crosslinking and an ultrathin electrolyte membrane with limited swelling was prepared.
It realizes an ultra-thin electrolyte membrane with mechanical stability and thickness controllability while maintaining high ion conductivity, improving the long-term performance and reliability of electrochemical devices, and is suitable for high-performance batteries and wearable devices.
Smart Images

Figure CN118983510A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an ultra-thin electrolyte membrane for a battery or other electrochemical devices and a preparation method and application thereof, belonging to the technical field of polymer materials. Background Art
[0002] In recent years, with the continuous increase in energy demand and the increasing attention to environmental protection, the development of new energy technologies has attracted much attention. Among the many new energy technologies, electrochemical energy storage such as batteries and supercapacitors have become a hot spot in research and application due to their high efficiency and environmental protection. One of its core components is the electrolyte membrane. The performance of the electrolyte membrane directly affects the working efficiency and stability of batteries and supercapacitors, so the preparation of high-performance electrolyte membranes has become one of the key areas of electrochemical energy storage research.
[0003] As a mature nanofiber preparation technology, electrospinning can produce ultrathin films with high porosity and large specific surface area. These characteristics make electrospinning technology the preferred method for preparing electrolyte membranes. Polymers such as polyvinylidene fluoride (PVDF) and polyvinyl alcohol (PVA) are widely used in the preparation of electrolyte membranes due to their good chemical stability, mechanical properties and ion affinity. Although the existing technology has made certain progress in the preparation of ultrathin electrolyte membranes, there are still some key problems that need to be solved: (1) Swelling problem: Hydrophilic polymers easily absorb water and swell in salt solutions, resulting in an increase in the thickness of the electrolyte membrane, which not only affects the volume energy density of the battery, but also may cause the mechanical properties of the membrane to decrease or even rupture. (2) Thickness control: It is difficult to achieve precise control of the thickness of the electrolyte membrane with the existing technology, especially after long-term immersion in salt solutions, the thickness and performance of the electrolyte membrane may change unpredictably. (3) Stability and durability: The swollen, thickened or dissolved electrolyte membrane will reduce the cycle stability and overall durability of the battery, affecting the long-term reliability and service life of the electrochemical energy storage device.
[0004] In view of the above problems, it is urgent to develop a new type of ultra-thin electrolyte membrane that can maintain high ion conductivity while having good thickness controllability, mechanical stability and chemical stability. This electrolyte membrane should be able to resist swelling caused by salt solutions and maintain the long-term performance and reliability of the battery. In addition, the new electrolyte membrane should also have good electrochemical stability and be able to work stably within a wide potential window. Summary of the invention
[0005] Purpose of the invention: The first purpose of the present invention is to provide a method for preparing an ultra-thin electrolyte membrane. The second purpose of the present invention is to provide a method for preparing the ultra-thin electrolyte membrane, which can produce an extremely thin electrolyte membrane with limited swelling, which is suitable for high-performance electrochemical devices. The third purpose of the present invention is to provide the ultra-thin electrolyte membrane for high-performance electrochemical devices.
[0006] Technical solution: The ultra-thin electrolyte membrane described in the present invention comprises a precursor polymer film in which hydrophobic and hydrophilic networks are uniformly dispersed by dissolving a hydrophobic polymer and a hydrophilic polymer simultaneously with a strong polar solvent, using electrospinning technology to prepare the precursor polymer film, immersing the precursor polymer film in a solution containing a cross-linking agent, using in-situ chemical cross-linking technology to prepare a polymer film with limited swelling, and immersing the polymer film in a salt solution to obtain the membrane.
[0007] Further, the hydrophobic polymer is selected from polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), polypropylene (PP), polyethylene (PE), polystyrene (PS), polytetrafluoroethylene (PTFE), polycarbonate (PC) or polymethyl methacrylate (PMMA).
[0008] Further, the hydrophilic polymer is selected from polyvinyl alcohol (PVA), polyethylene glycol (PEG), polyethylene oxide (PEO), poly(vinyl sulfonic acid) (PVS), polyvinyl pyrrolidone (PVP) or polyacrylic acid (PAA).
[0009] Furthermore, the strong polar solvent is selected from dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF), N-methylpyrrolidone (NMP), tetrahydrofuran (THF), dichloromethane (CH2Cl2), dimethylacetamide (DMAc) or acetone.
[0010] Furthermore, the crosslinking agent is selected from aldehyde compounds (Aldehydes), epoxides (Epoxides), isocyanates (Isocyanates), N,N-dimethylacrylamide (N,N-Dimethylacrylamide), boric acid (Boric Acid) or sodium tetraborate (Borax).
[0011] Furthermore, the aldehyde compound is glutaraldehyde, paraformaldehyde or glyoxal.
[0012] Furthermore, the epoxy compound is epichlorohydrin, ethylene oxide or butadiene monoxide.
[0013] Furthermore, the salt solution is a sodium salt solution, a potassium salt solution, a magnesium salt solution, an ammonium salt solution, a zinc salt solution or a lithium salt solution.
[0014] Furthermore, the sodium salt is sodium chloride (NaCl), sodium nitrate (NaNO3) or sodium sulfate (Na2SO4).
[0015] Furthermore, the potassium salt is potassium chloride (KCl), potassium nitrate (KNO3) or potassium sulfate (K2SO4).
[0016] Furthermore, the magnesium salt is magnesium chloride (MgCl2), magnesium nitrate (Mg(NO3)2) or magnesium acetate (Mg(OAc)2).
[0017] Furthermore, the ammonium salt is ammonium chloride (NH4Cl), ammonium sulfate ((NH4)2SO4) or ammonium nitrate (NH4NO3).
[0018] Furthermore, the zinc salt is zinc chloride (ZnCl2), zinc sulfate (ZnSO4), zinc perchlorate (Zn(ClO4)2), zinc trifluoromethanesulfonate (ZnOtf2) or zinc nitrate (Zn(NO3)2).
[0019] Furthermore, the lithium salt is lithium chloride (LiCl), lithium nitrate (LiNO 3 ) or lithium bis(trifluoromethanesulfonyl)imide (LiTFSI).
[0020] Furthermore, the thickness of the ultra-thin electrolyte membrane is less than 100 μm.
[0021] The method for preparing the ultrathin electrolyte membrane of the present invention comprises the following steps:
[0022] (1) dissolving a hydrophobic polymer powder and a hydrophilic polymer powder in a strong polar solvent to form a uniform solution;
[0023] (2) using electrospinning technology to prepare the solution obtained in step (1) into a precursor polymer film;
[0024] (3) immersing the precursor polymer film in a solution containing a crosslinking agent to perform a chemical crosslinking reaction, so that the hydrophilic polymer network forms a chemically crosslinked polymer film through the crosslinking agent;
[0025] (4) The chemically cross-linked polymer membrane is immersed in a salt solution to obtain an ultrathin electrolyte membrane through the restricted swelling of the hydrophilic polymer network.
[0026] Furthermore, in step (1), the solid-liquid ratio of the hydrophobic polymer powder, the hydrophilic polymer powder and the strong polar solvent is 0.01-0.5:0.01-0.5:1 g / g / mL.
[0027] Furthermore, in step (2), the parameters during electrospinning are: voltage 15-25 kV, needle distance 5-45 cm from the receiving point, injection speed 0.01-0.5 mm / min, and receiving speed 10-120 r / min.
[0028] Furthermore, in step (3), the mass ratio of the precursor polymer film to the cross-linking agent is 10000:1-100:1.
[0029] Furthermore, in step (3), the temperature of the chemical cross-linking reaction is 25-80° C., and the time of the chemical cross-linking reaction is 0.5-10 h.
[0030] Furthermore, in step (4), the concentration of the salt solution is 0.1-4 mol / L. Furthermore, in step (4), the treatment temperature is 25-60° C. and the treatment time is 1-24 h.
[0031] The present invention also includes the use of the ultra-thin electrolyte membrane in a high-performance electrochemical device.
[0032] Furthermore, the high-performance electrochemical device is a battery, a wearable device or a supercapacitor.
[0033] Principle of the invention: The present invention selects appropriate hydrophobic polymers and hydrophilic polymer networks, which play different roles in the electrolyte membrane. The hydrophobic network provides the basic mechanical strength and chemical stability of the electrolyte membrane, while the hydrophilic network is responsible for the conduction of ions. The hydrophilic network is formed into a chemically cross-linked network structure in the film through a cross-linking agent. Chemical cross-linking not only enhances the mechanical stability of the film, but also controls the thickness of the electrolyte membrane by limiting the swelling of the hydrophilic network. By adjusting the ratio of the hydrophobic polymer and the hydrophilic polymer and the amount of the cross-linking agent, the ionic conductivity and mechanical stability of the electrolyte membrane can be optimized to meet the requirements of high-performance electrochemical devices.
[0034] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages:
[0035] (1) The preparation method of the present invention is simple, the equipment requirements are low, the ultra-thin electrolyte membrane is foldable, and the thickness is less than 100 μm;
[0036] (2) The present invention uses chemical cross-linking and limited swelling technology to ensure that the electrolyte membrane has high ion conductivity while maintaining good mechanical stability, which is crucial for improving electrochemical performance;
[0037] (3) The ultrathin electrolyte membrane of the present invention is not only suitable for traditional battery technology, but can also be used in new flexible batteries, wearable devices and other high-performance electrochemical devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 This is a macroscopic photograph of the ultrathin electrolyte membrane obtained in Example 1;
[0039] Figure 2 is a SEM image of the ultrathin electrolyte membrane obtained in Example 1;
[0040] Figure 3 Ionic conductivity and mechanical properties of electrolyte membranes of different proportions in Example 2;
[0041] Figure 4 This is a diagram showing the thickness of the ultra-thin electrolyte membrane in Example 3;
[0042] Figure 5 The zinc stability curves of the zinc-zinc symmetric batteries prepared from the ultrathin electrolyte membrane in Example 4 and the non-crosslinked electrolyte membrane in Comparative Example 1;
[0043] Figure 6 This is a SEM image of the ammonium vanadate positive electrode used to assemble the zinc ion battery in Example 5;
[0044] Figure 7 This is a graph showing the charge and discharge cycle performance of a zinc ion battery based on a chemically cross-linked ultrathin electrolyte in Example 5;
[0045] Figure 8 This is a diagram showing the zinc ion battery based on chemically cross-linked ultrathin electrolyte in Example 5 powering a smartphone. DETAILED DESCRIPTION
[0046] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.
[0047] Example 1
[0048] Polyacrylonitrile (PAN) and polyvinyl alcohol (PVA) powders were used as hydrophobic and hydrophilic polymers. 0.916 g PAN powder and 0.916 g PVA powder were dissolved in 20 mL dimethyl sulfoxide (DMSO) and stirred at room temperature for 24 hours using a magnetic stirrer until a uniform solution was formed. The solution was loaded into a plastic syringe with a metal nozzle and electrospun for 6 hours using an electrospinning device (Beijing Yongkang Leye Technology Development Mailbox Company, ET-2) at 20 kV voltage and a push speed of 0.1 mm / min, a receiving speed of 100 r / min, and a needle distance of 25 cm from the receiving end to prepare a precursor polymer film. The precursor film was immersed in an aqueous solution containing a crosslinking agent, glyoxal (the concentration of the aqueous solution of glyoxal was 1 mol / L), and reacted at 40 ° C for 6 hours to form a chemically crosslinked polymer film. The chemically crosslinked film was immersed in a 1 mol / L zinc sulfate solution and treated at 25°C for 24 hours to complete the preparation of the chemically crosslinked ultrathin electrolyte membrane (Crosslinked PVA-PAN). The tensile strength at break of the chemically crosslinked ultrathin electrolyte membrane was tested to be 21.2 MPa.
[0049] Figure 1 This is a macroscopic photograph of the ultrathin electrolyte membrane obtained in Example 1. Figure 1 It can be seen that the electrolyte membrane is very thin and can be bent as a whole, and has good flexibility.
[0050] The thickness of the ultra-thin electrolyte membrane was tested using a scanning electron microscope. Figure 2 shown. Figure 2 This is a measurement diagram of the thickness of the ultra-thin electrolyte membrane. The thickness was measured to be 20.2μm using a scanning electron microscope.
[0051] Comparative Example 1
[0052] The preparation process is the same as in Example 1, except that polyacrylonitrile (PAN) and polyvinyl alcohol (PVA) powders are taken as hydrophobic and hydrophilic polymers without crosslinking by a crosslinking agent. 0.916g PAN and 0.916g PVA powders are dissolved in 20ml dimethyl sulfoxide (DMSO) and stirred at room temperature for 24 hours using a magnetic stirrer until a uniform solution is formed. The solution is loaded into a plastic syringe with a metal nozzle, and an electrospinning device is used to prepare a non-precursor polymer film at a voltage of 20kV and a push injection speed of 0.1mm / min, a receiving speed of 100r / min, and a needle distance of 25cm from the receiving place, and electrospinning for 6h. The precursor polymer film is immersed in a 1mol / L zinc sulfate solution and treated at 25°C for 24 hours to obtain an electrolyte membrane that is not chemically crosslinked (PVA-PAN that is not chemically crosslinked). The tensile strength of the electrolyte membrane that is not chemically crosslinked is tested to be 9.8MPa. It is shown that the tensile strength of the electrolyte membrane can be significantly indicated after crosslinking by a crosslinking agent.
[0053] Example 2
[0054] The preparation process is the same as that in Example 1, except that the mass ratio of PVA and PAN is adjusted to 1:1, 2:1 and 1:2, respectively, to study the effects of different ratios on the performance of the electrolyte membrane. PVA and PVDF are dissolved in DMF according to the selected ratio to form a uniform mixed solution. Precursor polymer films of different proportions are prepared using the electrospinning technology of Example 1. An aqueous solution of paraformaldehyde is selected as a cross-linking agent (the concentration of the aqueous solution of paraformaldehyde is 1 mol / L), the film is immersed in the cross-linking agent solution, and reacted at 50°C for 6 hours to form a chemically cross-linked polymer film. The chemically cross-linked film is immersed in a 1 mol / L zinc sulfate solution and treated at 60°C for 24 hours to complete the preparation of the ultra-thin electrolyte membrane.
[0055] The electrolyte membranes prepared in this example with different ratios were tested for ion conductivity and mechanical properties to determine the optimal ratio. Figure 3 As shown. Figure 3 It can be seen that considering the mechanical properties and ion transmission capacity comprehensively, the optimal mass ratio of PVA and PAN is 1:1.
[0056] Example 3
[0057] The preparation process is the same as that in Example 1, except that a flexible hydrophobic polymer such as polyimide (PI) is selected instead of PAN to improve the flexibility of the electrolyte membrane. PI and PVA are dissolved in an appropriate solvent, such as N-methylpyrrolidone (NMP), to form a uniform mixed solution. The precursor polymer film is prepared by electrospinning for 5 hours at a voltage of 20.5 kV and a push speed of 0.2 mm / min, a receiving speed of 120 r / min, and a needle distance of 25 cm from the receiving point. The precursor film is immersed in an aqueous solution containing a cross-linking agent glutaraldehyde (the concentration of the aqueous solution of glutaraldehyde is 1 mol / L), and reacted at 40°C for 6 hours to form a chemically cross-linked polymer film. The cross-linked film is immersed in a lithium bis(trifluoromethanesulfonyl)imide solution and treated at 60°C for 24 hours to obtain an ultra-thin electrolyte membrane suitable for flexible batteries. The optical photograph is as shown Figure 4 As shown, the thickness is only 66 microns.
[0058] Example 4
[0059] A zinc-zinc symmetric battery was prepared using the chemically cross-linked ultrathin electrolyte membrane Crosslinked PVA-PAN prepared in Example 1 and the non-chemically cross-linked PVA-PAN membrane prepared in Comparative Example 1: 1 cm×1 cm square zinc foil was used as the two electrodes of the zinc-zinc symmetric battery, the chemically cross-linked ultrathin electrolyte membrane Crosslinked PVA-PAN and the non-chemically cross-linked PVA-PAN membrane (1.2 cm×1.2 cm) were used as electrolytes, and sandwich-structured zinc-zinc symmetric batteries were assembled respectively.
[0060] The voltage polarization curves of Zn / / Crosslinked PVA-PAN / / Zn and Zn / / PVA-PAN / / Zn were analyzed for the stability of zinc. Figure 5 shown. Figure 5 The zinc stability curves of the zinc-zinc symmetric battery prepared by the ultrathin electrolyte membrane in Example 4 and the uncrosslinked electrolyte membrane in Comparative Example 1 are shown in FIG. Figure 5 It can be seen that at 0.1 mA cm -2 At a current density of 1.5 , the chemically cross-linked ultra-thin electrolyte film Crosslinked PVA-PAN can stably cycle for 1200 hours, while the film without chemical cross-linking has an abnormal curve after 50 hours, showing obvious uneven deposition and short-circuit behavior, that is, battery failure. The chemically cross-linked electrolyte film has excellent zinc stability and calendar life.
[0061] Example 5
[0062] The chemically crosslinked ultrathin electrolyte membrane Crosslinked PVA-PAN prepared in the embodiment and the non-chemically crosslinked PVA-PAN membrane obtained in the comparative example 1 were used to prepare zinc ion batteries: ammonium vanadate was used as the active material, acetylene black was used as the conductive agent, PVDF was used as the binder, and the stainless steel mesh was used as the current collector. 140 mg of the ground ammonium vanadate material was mixed with 40 mg of acetylene black and 10 mg of PVDF in a mass ratio of 7:2:1, and mixed evenly using a ball mill, and then coated on a stainless steel mesh (10 cm×10 cm), and the active material surface loading was 0.7-1.4 mg / cm 2 The positive electrode of zinc ion battery is obtained by cutting it into a square electrode sheet of 3cm×3cm. Figure 6 As shown. A 3.5cm×3.5cm square zinc foil was used as the negative electrode of the zinc ion battery, and a chemically crosslinked ultrathin electrolyte membrane Crosslinked PVA-PAN and a non-chemically crosslinked PVA-PAN membrane (4cm×4cm) were used as electrolytes to assemble sandwich structure zinc ion batteries. The cycle performance of the battery is shown in Figure 7 As shown by Figure 7 It can be seen that 10Ag -1 At a current density of 1.3 Å, the chemically crosslinked electrolyte membrane CrosslinkedPVA-PAN can stably cycle for 1000 cycles, while the electrolyte membrane without chemical crosslinking rapidly decays to 10 mAh g after 300 cycles. -1 .
[0063] According to the above method, four zinc-ion batteries based on chemically cross-linked ultrathin electrolyte membranes are connected in series, such as Figure 8 As shown, it can power a smartphone.
[0064] Example 6
[0065] The preparation process is the same as that of Example 1, except that the hydrophobic polymer is selected from PVDF, PAN, PP, PE, PS, PTFE, PC or PMMA; the hydrophilic polymer is selected from PVA, PEG, PEO, PVS, PVP or PAA; the polar solvent is selected from DMSO, DMF, NMP, THF, CH2Cl2, DMAc or Acetone; the crosslinking agent is selected from Glutaraldehyde, Aldehydes, Epoxides, Isocyanates, N,N-Dimethylacrylamide, Boric Acid or Borax; the salt solution is a sodium salt, potassium salt, magnesium salt, ammonium salt, zinc salt or lithium salt solution; the electrospinning voltage is 15-25 kV; the crosslinking time is 0.5-10 h, as shown in Table 1. As can be seen from Table 1, the ultra-thin electrolyte membrane can reach less than 100 microns at this time.
[0066] Table 1
[0067]
[0068]
Claims
1. An ultra-thin electrolyte membrane, It is characterized in that The ultra-thin electrolyte membrane comprises dissolving a hydrophobic polymer and a hydrophilic polymer simultaneously by a strong polar solvent, preparing a precursor polymer film with a uniformly dispersed hydrophobic and hydrophilic network by using an electrospinning technique, immersing the precursor polymer film in a solution containing a cross-linking agent, preparing a polymer film with limited swelling by using an in-situ chemical cross-linking technique, and immersing the polymer film in a salt solution.
2. The ultrathin electrolyte membrane according to claim 1, It is characterized in that The hydrophobic polymer is selected from polyvinylidene fluoride, polyacrylonitrile, polypropylene, polyethylene, polystyrene, polytetrafluoroethylene, polycarbonate or polymethyl methacrylate.
3. The ultrathin electrolyte membrane according to claim 1, It is characterized in that The hydrophilic polymer is selected from polyvinyl alcohol, polyethylene glycol, polyethylene oxide, poly(vinyl sulfonic acid), polyvinyl pyrrolidone or polyacrylic acid.
4. The ultrathin electrolyte membrane according to claim 1, It is characterized in that The strong polar solvent is selected from dimethyl sulfoxide, N,N-dimethylformamide, N-methylpyrrolidone, tetrahydrofuran, dichloromethane, dimethylacetamide or acetone.
5. The ultrathin electrolyte membrane according to claim 1, It is characterized in that The crosslinking agent is selected from aldehyde compounds, epoxy compounds, isocyanate, N,N-dimethylacrylamide, boric acid or sodium tetraborate.
6. The ultrathin electrolyte membrane according to claim 1, It is characterized in that The salt solution is a sodium salt solution, a potassium salt solution, a magnesium salt solution, an ammonium salt solution, a zinc salt solution or a lithium salt solution.
7. The ultrathin electrolyte membrane according to claim 1, It is characterized in that The thickness of the ultra-thin electrolyte membrane is less than 100 μm.
8. A method for preparing an ultrathin electrolyte membrane according to any one of claims 1 to 7, It is characterized in that The following steps are involved: (1) dissolving a hydrophobic polymer powder and a hydrophilic polymer powder in a strong polar solvent to form a uniform solution; (2) using electrospinning technology to prepare the solution obtained in step (1) into a precursor polymer film; (3) immersing the precursor polymer film in a solution containing a crosslinking agent to perform a chemical crosslinking reaction, so that the hydrophilic polymer network forms a chemically crosslinked polymer film through the crosslinking agent; (4) The chemically cross-linked polymer membrane is immersed in a salt solution to obtain an ultrathin electrolyte membrane through the restricted swelling of the hydrophilic polymer network.
9. The method for preparing the ultrathin electrolyte membrane according to claim 8, It is characterized in that In step (1), the solid-liquid ratio of the hydrophobic polymer powder, the hydrophilic polymer powder and the strong polar solvent is 0.01-0.5:0.01-0.5:1 g / g / mL. In step (2), the parameters during electrospinning are: voltage 15-25 kV, needle distance 5-45 cm from the receiving end, injection speed 0.01-0.5 mm / min, receiving speed 10-120 r / min. In step (3), the mass ratio of the precursor polymer film to the cross-linking agent is 10000:1-100:1, the temperature of the chemical cross-linking reaction is 25-80°C, and the time of the chemical cross-linking reaction is 0.5-10 h. In step (4), the concentration of the salt solution is 0.1-4 mol / L, the temperature during treatment is 25-60°C, and the time during treatment is 1-24 h.
10. The ultra-thin electrolyte membrane according to any one of claims 1 to 7 is used in a high-performance electrochemical device.