Method and device for purifying titanic acid
Through reverse washing technology and stirring treatment, the quality unstable and wastewater problems in titanium dioxide production are solved, and efficient, low-consumption and environmentally friendly titanium dioxide production is achieved, reducing production costs and environmental pollution.
Patent Information
- Application Number
- CN202411020683.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-22
AI Technical Summary
The existing titanium dioxide production process has problems such as unstable product quality, high energy consumption, large wastewater discharge and high environmental protection pressure, making it difficult to obtain high-purity and stable quality titanium dioxide.
Using the reverse washing technology, the impurity-containing metatitanic acid is added to the washing parts from top to bottom, and the washing liquid flows from bottom to top. Through countercurrent contact and gravity settlement, soluble impurities are removed, combined with stirring and temperature control, and water consumption and wastewater discharge are reduced.
The stable production of high-quality titanium dioxide has been achieved, reducing the pure water consumption per ton of product by 30-45m³, reducing production costs by about 800 yuan, reducing the "three wastes" emissions, and improving the environmental protection effect.
Smart Images

Figure CN118988543A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method and a device for purifying titanic acid, and in particular to a method and a device for purifying titanic acid with high efficiency and environmental protection. Background Art
[0002] Titanium dioxide is an important inorganic chemical pigment, the main component of which is titanium dioxide. There are two production processes for titanium dioxide: sulfuric acid process and chlorination process. It has important uses in industries such as coatings, inks, papermaking, plastics and rubber, chemical fibers, and ceramics.
[0003] At present, various manufacturers use the method of hydrolyzing titanium sulfate to generate metatitanic acid. After the metatitanic acid is filtered by a filter, it is washed with a large amount of water in the filter to produce a product that meets the requirements of the finished product. This refining process consumes 50m³ of desalted water for each ton of product, and also produces a large amount of wastewater. Even so, the quality of the products produced cannot be stable, and the product quality of each filter will fluctuate. In addition, due to the presence of ferrous salts, each time the washing is switched, the ferrous salts will be oxidized and discolored, and the ferrous salts must be reduced and decolorized. The above-mentioned traditional refining process cannot obtain high-purity titanium dioxide products, nor can it obtain titanium dioxide products of stable quality. However, it has obvious disadvantages such as difficulty in ensuring stable product quality, high energy consumption, large wastewater discharge, and high environmental pressure. This traditional purification process with high energy consumption, large wastewater volume, and unstable quality is in urgent need of appropriate improvement and improvement in the current situation of advocating "high efficiency, high quality, low consumption, and environmental protection". Summary of the invention
[0004] The purpose of the present invention is to provide a high-efficiency method for purifying metatitanic acid (titanium hydroxide) in view of the shortcomings of the existing purification process in the titanium dioxide production process, so as to improve the quality of the titanium dioxide product, reduce water consumption, reduce wastewater discharge, improve product quality, reduce energy consumption, reduce production costs, and reduce environmental protection treatment costs.
[0005] The technical solution to solve the technical problem of the present invention is that a method for purifying titanic acid includes reverse washing, upper liquid discharge, and lower purified material discharge; In the reverse washing, the impure metatitanic acid is added from top to bottom into the liquid in the washing component, and the washing liquid is added from bottom to top into the washing component, the impure metatitanic acid contacts with the washing liquid in countercurrent, and falls to the bottom of the washing component by gravity sedimentation of the metatitanic acid, the washing liquid injected from the bottom is mixed and washed with the impure metatitanic acid, and the washing liquid extracts the soluble impurities mixed with the metatitanic acid, and the stirring component stirs the inside of the washing component; The upper liquid is discharged, and the washing liquid containing impurities overflows and is discharged from the top of the washing component; The purified material in the lower part is discharged, and the titanic acid with soluble impurities removed sinks to the lower part of the washing part under the action of gravity and is discharged.
[0006] Furthermore, in the reverse washing process, the washing liquid is added from a position at least one meter away from the bottom of the washing component.
[0007] Furthermore, during the reverse washing process, the titanic acid addition port is at least 20 cm below the overflow port, and preferably 3-5 m below the overflow port.
[0008] Furthermore, during the reverse washing process, the internal temperature of the washing component is controlled at 0°C-100°C.
[0009] Furthermore, the washing liquid is water or a water-alcohol mixture, and the mass ratio of the water-alcohol mixture is 9:1-1:9.
[0010] Furthermore, the water-to-alcohol mass ratio is preferably 1:1-2:1.
[0011] Furthermore, the volume ratio of the impure titanic acid to the washing liquid is 1:1-1:20.
[0012] A titanate purification device comprises a scrubber, wherein a solid feed pipe and a liquid discharge pipe are arranged at the upper part of the scrubber, a scrubbing liquid inlet pipe is arranged at the lower part of the scrubber, and a purified product discharge pipe is arranged at the bottom of the scrubber; A stirring component is arranged in the scrubber.
[0013] Further, the scrubber is one of a rotary disc type and a pulse tower.
[0014] Furthermore, the solid feed pipe extends into the interior of the scrubber and is perpendicular to the orthographic projection plane of the scrubber.
[0015] The advantages of the present invention are: 1. The method of the present invention can obtain stable and high-quality titanium dioxide.
[0016] 2. Reduce the amount of pure water used by 30-45m³ per ton of product, and also greatly reduce wastewater discharge.
[0017] 3. Save energy and reduce consumption, achieve low-cost production of high-quality titanium dioxide, and reduce production costs by about RMB 800 per ton of product.
[0018] 4. The new purification process can reduce the emission of "three wastes" and environmental pollution. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a logic block diagram of the method of the present invention.
[0020] Figure 2It is a schematic diagram of the structure of the device of the present invention.
[0021] As shown in the figure, there are a scrubber 1, a solid feed pipe 2, a liquid discharge pipe 3, a washing liquid inlet pipe 4, a purified product discharge pipe 5, a stirring component 6, titanic acid A, a washing component B, a washing liquid C, and a stirring component E. DETAILED DESCRIPTION
[0022] The impurities contained in the impurity-containing metatitanic acid (titanium hydroxide) are mainly water-soluble impurities, such as ferrous sulfate, sulfuric acid, zirconium sulfate, aluminum sulfate, magnesium sulfate, calcium sulfate, sodium sulfate, potassium sulfate and other soluble impurities. These impurities have a relatively large impact on the quality of titanium dioxide. For example, iron salts will reduce whiteness, and zirconium will increase the gloss and saturation of titanium, but will reduce its antioxidant properties. Through a large amount of water washing, the water-soluble impurities are separated from the metatitanic acid (titanium hydroxide). The main indicators improved by water washing are: TiO2 (W%): mass percentage content of titanium dioxide: whiteness: smaller fluctuations in the pH range: reduced volatile matter at 105°C: increased resistivity and reduced water-soluble matter (W%). The present invention can greatly reduce the amount of water used for washing by improving the washing method and device, while ensuring the washing effect.
[0023] like Figure 1 As shown in, the method for purifying titanic acid includes reverse washing, upper liquid discharge, and lower purified material discharge; In the reverse washing, the impurity-containing metatitanic acid A is added from top to bottom into the liquid in the washing part B, and the washing liquid C is added from bottom to top into the washing part B. The impurity-containing metatitanic acid A contacts with the washing liquid C in countercurrent flow, and falls to the bottom of the washing part B by gravity sedimentation of the metatitanic acid. The washing liquid injected from the bottom is mixed and washed with the impurity-containing metatitanic acid, and the washing liquid extracts the soluble impurities mixed with the metatitanic acid. The stirring part E stirs the inside of the washing part B. The upper liquid is discharged, and the washing liquid containing impurities overflows and is discharged from the top of the washing part B; The purified material in the lower part is discharged, and the titanic acid with soluble impurities removed sinks to the lower part of the washing part B under the action of gravity and is discharged.
[0024] Preferably, during the reverse washing process, the washing liquid is added from a position at least 20 cm away from the bottom B of the washing component.
[0025] Preferably, during the reverse washing process, the internal temperature of the washing component is controlled at 0°C-100°C, and further controlled at 20°C-60°C, and the pressure can be normal pressure, high pressure, or negative pressure.
[0026] Preferably, the washing liquid is water or a water-alcohol mixture, and the mass ratio of the water-alcohol mixture washing liquid is 1:9-9:1.
[0027] Preferably, the water-to-alcohol mass ratio is 1:1-2:1.
[0028] Preferably, the volume ratio of the impure metatitanic acid to the washing liquid is 1:5-1:20, preferably 1:5-10.
[0029] like Figure 2 A titanate purification device comprises a scrubber 1, a solid feed pipe 2 and a liquid discharge pipe 3 are provided at the upper part of the scrubber 1, a scrubbing liquid inlet pipe 4 is provided at the lower part of the scrubber 1, and a purified product discharge pipe 5 is provided at the bottom of the scrubber 1; A stirring component 6 is provided in the scrubber 1 .
[0030] Preferably, the scrubber 1 is a rotary disc tower or a pulse tower.
[0031] Preferably, the solid feed pipe 2 extends into the interior of the scrubber 1 and is perpendicular to the orthographic projection plane of the scrubber 1 , that is, perpendicular to the installation surface of the scrubber 1 .
[0032] During operation, washing liquid is first introduced into the scrubber 1, and then the impure titanic acid enters the washing liquid in the scrubber 1 through the solid feed pipe 2, and moves from top to bottom under the action of gravity. During its movement, the washing liquid extracts the soluble impurities mixed with the titanic acid. The washing liquid is continuously injected into the scrubber 1 from the washing liquid inlet pipe 4, and discharged from the liquid discharge pipe 3 of the scrubber 1. After discharge, it is connected to the liquid treatment device to treat the soluble impurities therein. The extracted titanic acid falls to the bottom of the scrubber 1 and is discharged through the purified product discharge pipe 5.
[0033] Embodiment 1: After hydrolysis of titanyl sulfate, the dilute acid content is 200g / L, the ferrous content is 5g / L, 10L of metatitanic acid is taken for pulping, and 50L of washing pure water is taken, the temperature is 25°C, and the pH value is 6.8.
[0034] 1) From Figure 2 , fill the washing liquid inlet pipe 4 of the scrubber 1 with pure water, and start overflowing from the liquid discharge pipe 3. The water inlet speed at the bottom is adjusted by the flow meter through the valve to control the flow rate: 10 liters / h.
[0035] 2) Start Figure 2 The variable frequency reduction motor with a main shaft speed of 50 rpm causes the stirring component 6 to rotate in the scrubber 1.
[0036] 3) 10 liters of metatitanic acid, Figure 2 The solid feed pipe 2 of the scrubber 1 begins to continuously feed, and the flow rate is controlled to continuously feed 10 liters of titanic acid for four hours.
[0037] 4) From Figure 2 The discharge rate of the purified product discharge pipe 5 of the scrubber 1 is controlled at 4 liters / h, concentration 50%. 5) The scrubber implemented has a diameter of 80 mm and a height of 2000 mm, and the overflow port n2 is 300 mm above the n1 feed port.
[0038] 6) The upward flow velocity of the liquid in the scrubber washing section is V1 = 2.4 mm / s, and the solid settling velocity is V2 = 1 mm / s. The liquid rising velocity in the top settling section is V3 = 0.47 mm / s.
[0039] 7) After 0.6 hours, samples were taken from the three outlets of the liquid discharge pipe, and 400 ml of samples were taken continuously for four time periods, namely 0.6-0.7h, 0.7-0.8h, 0.8-0.9h, and 0.9-1h; 8) The four samples were vacuum filtered and dehydrated, and then dried in an oven at 105°C for 4 hours. The weights of the samples in the three intervals were obtained: 205.5 g, 204.6 g, 203.8 g, and 203.1 g.
[0040] 9) Sample pH and ferrous content analysis
[0041] Embodiment 2: After hydrolysis of titanyl sulfate, the dilute acid content is 200g / L, the ferrous content is 5g / L, the moisture content of 10 liters of metatitanic acid is about 80%, the washing liquid is an aqueous solution containing 30% methanol, the temperature is 25°C, and the pH value is 6.8.
[0042] 1) From Figure 2 The washing liquid inlet pipe 4 is filled with pure water, and begins to overflow from the liquid discharge pipe 3. The water inlet speed at the bottom is adjusted by the flow meter to control the flow rate: 10 liters / h.
[0043] 2) Start Figure 2 The variable frequency reduction motor with a main shaft speed of 50 rpm causes the stirring component 6 to rotate in the scrubber 1.
[0044] 3) 10 liters of titanic acid are continuously added through the second port of the solid feed pipe, and the addition of 10 liters is completed continuously within four hours by flow control.
[0045] 4) From Figure 1 The discharge volume of the three outlets of the liquid discharge pipe at the bottom is controlled at 4 liters / h, concentration 50%. 5) The scrubber implemented has a diameter of 80 mm and a height of 2000 mm, and the overflow port n2 is 300 mm above the n1 feed port.
[0046] 6) The upward flow velocity of the liquid in the scrubber washing section is V1 = 2.4 mm / s, and the solid settling velocity is V2 = 1.68 mm / s. The liquid rising velocity in the top settling section is V3 = 0.47 mm / s.
[0047] 7) After 0.4 hours, samples were taken from the 5 ports of the purified product discharge tube, and 400 ml of each sample was taken continuously for 4 time periods, namely 0.6-0.7h, 0.7-0.8h, 0.8-0.9h, and 0.9-1h; 8) The four samples were vacuum filtered and dehydrated, and then dried in an oven at 105°C for 4 hours. The weights of the samples in the three intervals were obtained: 206.5 g, 204.9 g, 204.8 g, and 204.1 g.
[0048] 9) Sample pH and ferrous content analysis
Claims
1. A method for purifying titanic acid, characterized in that: The method comprises reverse washing, upper liquid discharge, and lower purified material discharge; In the reverse continuous washing, the impure metatitanic acid is added from top to bottom into the liquid in the washing part, and the washing liquid is added from bottom to top into the washing part, the impure metatitanic acid contacts with the washing liquid in countercurrent, and falls to the bottom of the washing part by gravity sedimentation of the metatitanic acid, and the washing liquid injected from the bottom is mixed and washed with the impure metatitanic acid, and the washing liquid extracts the soluble impurities mixed with the metatitanic acid, and the stirring part stirs the inside of the washing part; The upper liquid is discharged, and the washing liquid containing impurities overflows and is discharged from the top of the washing component; The purified material in the lower part is discharged, and the titanic acid with soluble impurities removed sinks to the lower part of the washing part under the action of gravity and is discharged.
2. The method for purifying titanic acid according to claim 1, characterized in that: In the reverse washing process, the washing liquid is added from a point at least 20 cm away from the bottom of the washing part.
3. The method for purifying titanic acid according to claim 1, characterized in that: During the reverse washing process, the density of the washing liquid is less than the density of metatitanic acid.
4. The method for purifying titanic acid according to claim 1, characterized in that: During the reverse washing process, the internal temperature of the washing part is controlled at 0°C-100°C.
5. A method for purifying titanic acid according to any one of claims 1 to 4, characterized in that: The washing liquid is water or a mixture of water and other solvents, and the mass ratio is 4:6-9.8:0.
2.
6. The method for purifying titanic acid according to claim 5, characterized in that: The water-to-alcohol mass ratio is 9:1-1:
9.
7. A method for purifying titanic acid according to any one of claims 1 to 4, characterized in that: The volume ratio of the impure titanic acid to the water washing liquid is 1:1-1:
20.
8. A device for purifying titanic acid, characterized in that: The device comprises a scrubber, wherein a solid feed pipe and a liquid discharge pipe are provided at the upper part of the scrubber, a scrubbing liquid inlet pipe is provided at the lower part of the scrubber, and a purified product discharge pipe is provided at the bottom of the scrubber; A stirring component is arranged in the scrubber.
9. The device for purifying titanic acid according to claim 8, characterized in that: The scrubber is a rotating disc or pulse tower.
10. The device for purifying titanic acid according to claim 8, characterized in that: The solid feed pipe extends into the interior of the scrubber and is perpendicular to the positive projection plane of the scrubber.
Citation Information
Cited By
Metatitanic acid continuous purifying and bleaching integrated method for dynamic reaction zone
CN121536956A